Novel sol resin slurry and preparation method thereof
By adding core-shell modified nanospheres and composite superabsorbent resin to epoxy resin slurry, a core-shell structure and cross-linking network are formed, which solves the problems of toughness and impact resistance of epoxy resin slurry and achieves better water plugging and seepage prevention effect and durability.
Patent Information
- Application Number
- CN202411225673.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Epoxy resin grout has poor toughness and impact resistance, and is prone to cracking and peeling under external pressure, affecting its water-blocking and seepage prevention effect.
Core-shell modified nanospheres and composite superabsorbent resin are added to epoxy resin slurry to enhance toughness and impact resistance by forming a core-shell structure and cross-linking network. Oxalic acid is used as a curing solvent to accelerate the curing process.
It significantly improves the water-blocking and seepage prevention effect, enhances the durability and toughness of epoxy resin, ensures stable existence under pressure and effectively prevents water flow, and reduces cracking and peeling.
Smart Images

Figure CN118931114A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of engineering water blocking and anti-seepage grouting, and specifically refers to a novel sol resin slurry and a preparation method thereof. Background Art
[0002] With the modernization of our country, rail facilities and infrastructure are developing in a large-scale and in-depth direction, and urban underground structures are also being constructed rapidly. As a result, the problem of underground structure leakage is becoming more and more frequent, causing the deterioration of the environment inside underground buildings and the reduction of structural durability, which seriously affects the appearance and various functions of the structure, and also has an adverse impact on its safety, durability and applicability. In order to ensure the safe and normal use of underground buildings, they must be plugged. Grouting plugging is the most commonly used method to control underground structure leakage. The basic mechanism of grouting plugging is to inject slurry into the leakage channel through grouting equipment, and the leakage channel is blocked by the slurry adhering, solidifying and filling in the channel, thereby achieving a good plugging effect.
[0003] At present, in addition to cement-based materials, organic polymer materials have been the research focus of grouting and plugging materials in recent years. Among them, epoxy resin grouting materials have the advantages of high bonding strength, high mechanical strength, excellent stability, curability at room temperature, and low shrinkage after curing. They have excellent application effects in repairing cracks and strengthening building structures.
[0004] The existing technology currently has the following problems:
[0005] Epoxy resin slurry has poor toughness and impact resistance, and is prone to cracking and falling off under the influence of external pressure. It is also not conducive to long-term stable use in practical applications, thus affecting the water blocking and anti-seepage effect. Summary of the Invention
[0006] In view of the above situation, in order to overcome the defects of the prior art, the present invention proposes a new sol resin slurry, comprising the following components in parts by weight: 60-90 parts of component A and 20-30 parts of component B.
[0007] The component A comprises the following components in parts by weight: 80-100 parts of epoxy resin slurry, 10-20 parts of core-shell nano-modified microspheres, 10-20 parts of composite super absorbent resin, and 5-8 parts of surfactant.
[0008] The B component is a solidifying solvent formed by dissolving oxalic acid in ethylene glycol solution.
[0009] Preferably, the method for preparing the core-shell nano-modified microspheres specifically comprises the following steps:
[0010] (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 50-100 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a hydrochloric acid solution with a mass fraction of 5.0-10.0%, ultrasonicate for 25-45 minutes, heat to 40-50 ° C, react for 1-2 hours, centrifuge to obtain a precipitate, and wash it with anhydrous ethanol 3-5 times, and vacuum dry. KH-570 forms an organic adsorption layer on the surface of the silica particles through its hydrolyzed group, thereby improving the dispersibility and stability of silica, and also improving the disadvantage of silica being brittle at low temperatures, thereby obtaining modified silica;
[0011] (2) Add 0.7g of Span 80 and 0.2g of Tween 60 to 30.0g of liquid paraffin, stir until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0g of acrylic acid, 4.0g of acrylamide, 0.55g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015g of N,N-methylenebisacrylamide to 20.0g of water, stir until completely dissolved, adjust the pH to 7.0 with a 5.0% sodium bicarbonate solution, and use as the water phase. At 40-50°C, dissolve 0.008g of ammonium persulfate and 0.008g of sodium bisulfite in 1-2mL of distilled water, and then add dropwise to the three-necked flask. Then add the oil phase. The phase and the aqueous phase are mixed, stirred evenly and poured into a flask, deoxygenated with nitrogen, stirred for 10-15 minutes and then continued to react for 3-4 hours. The crude product is obtained by demulsification, filtration and centrifugation, and washed with anhydrous ethanol for 3-5 times and vacuum dried. The modified nano-microspheres prepared by this method have a special core-shell structure. The polymer flexible shell on the surface of the microsphere absorbs water and swells, and is retained by adsorption, capture, bridging and the like. The rigid core is blocked in the pores. The synergistic effect of the two effectively prevents the flow of water and achieves the purpose of water blocking and anti-seepage. The microsphere structure also has good stability and durability, can exist stably in water, and can break through and advance under pressure, thereby enhancing the effect of water blocking and anti-seepage, and obtaining core-shell nano-modified microspheres;
[0012] Preferably, in step (2), the amount of modified silica added is 0.7-0.8 g. When subjected to impact, the modified silica can absorb part of the energy, reduce the generation and expansion of cracks, and enhance the mechanical properties and compatibility of the microspheres while synergizing with the microspheres to improve the impact resistance and toughness of the epoxy resin.
[0013] Preferably, the preparation method of the composite super absorbent resin specifically comprises the following steps:
[0014] a. Add 1.0 g of montmorillonite to 100 mL of water, stir at a speed of 100-300 rpm for 8-12 hours, then place it in an ultrasonic cell disruptor and ultrasonicate it at a power of 350-450 W for 3-5 minutes. Through ultrasonic treatment, the multi-layer montmorillonite is mechanically exfoliated into a low-dimensional structure with a large specific surface area and abundant active sites. Then, 0.1 g of octadecyltrimethylammonium bromide is added and stirred at 40-50 ° C for 3-5 hours. The montmorillonite after dimensionality reduction is washed with anhydrous ethanol, added to 200 mL of water and stirred. The mechanical and chemical exfoliation treatment method effectively destroys the multi-layer structure of the montmorillonite and decomposes it into a low-dimensional or even single-layer lamellar structure, which can be used for nano-blocking materials to obtain a nano-montmorillonite suspension.
[0015] b. Add 0.2 mL of a 1.0-2.0% mass fraction of 3-aminopropyltriethoxysilane aqueous solution dropwise to the nano-montmorillonite suspension described in step a at a constant temperature of 50° C. and stir thoroughly for 24 hours. After the reaction is completed, centrifuge at a speed of 5000 rpm for 3-5 minutes, wash the precipitate with anhydrous ethanol 3-5 times, and vacuum dry. The montmorillonite after amination treatment further enhances the adsorption capacity and stability of the montmorillonite by introducing amino groups, effectively absorbs and fixes water, reduces the flow and penetration of liquids, and has excellent water blocking and anti-seepage effects, thereby obtaining aminated montmorillonite;
[0016] c. 8.0 g starch and 2.0 g amination montmorillonite described in step b were added to 50 mL water and gelatinized at a constant temperature of 50-60 ° C for 0.5-1 h. The mixture was set aside. 5.0 g acrylic acid was weighed and placed in a conical flask containing 20 mL distilled water. 10-20 mL of sodium hydroxide solution with a mass fraction of 10% was added dropwise under an ice-water bath. 1.0 g of 2-acrylamide-2-methylpropanesulfonic acid was added after neutralization and stirred evenly. The mixture was set aside as a monomer. 0.7 g of Span 80 and 0.2 g of Tween 60 were added to 30.0 g of liquid paraffin. The mixture was mechanically stirred at a constant temperature of 45-55 ° C for 0.5-1 h. After forming a stable oil phase, the starch and amination montmorillonite solution were slowly added to the oil phase, emulsified at 45-55 ° C for 0.5-1 h. Finally, monomers, 2.0 g of potassium persulfate, 0.04 g of N,N-methylenediamine were added in sequence. Bisacrylamide is first degassed using an ultrasonic device. Degassing can prevent the formation of large pore structures and is conducive to the formation of uniform pore structures, thereby exhibiting good elasticity and strength, improving the toughness and impact resistance of the resin, and enhancing its durability. The product is then stirred and reacted at 45-55°C for 2-3 hours. The product is cooled to room temperature and washed with distilled water 3-5 times, vacuum filtered, dried, and crushed. A composite resin prepared from starch and modified montmorillonite as raw materials, vinyl monomer, and acrylic acid has high water absorption and swelling properties and excellent adhesion. When used in cracks and penetration areas, it will adhere to the surrounding building materials, absorb overflowing water, cause its own volume to expand, and thus fill cracks and pores. Its excellent adhesion ability effectively reduces the scouring of water or other factors, reduces loss or movement, and enhances the sealing effect to obtain a composite superabsorbent resin.
[0017] Preferably, in step a, the amount of octadecyltrimethylammonium bromide added is 1.0 g. Octadecyltrimethylammonium bromide achieves the effect of fully hydrating and dispersing montmorillonite through chemical exfoliation, further reducing the dimension of the montmorillonite structure.
[0018] The present invention also provides a method for preparing a novel sol resin slurry, which specifically comprises the following steps:
[0019] S1, 100g epoxy resin is dissolved in 10mL butyl glycidyl ether to form an epoxy resin slurry, and then core-shell nano-modified microspheres, composite super absorbent resin and surfactant are added thereto, and stirred evenly. The core-shell nano-modified microspheres and the composite super absorbent resin have good compatibility and can be evenly dispersed in the epoxy resin slurry. Due to the addition of the spherical structure and the cross-linked network structure of the composite resin, the toughness and impact properties of the epoxy resin are improved, and the water absorption and swelling capacity are enhanced. Among them, the core-shell nano-modified microspheres make up for the pressure bearing capacity of the composite super absorbent resin, and the composite super absorbent resin further enhances the water absorption and stability of the core-shell nano-modified microspheres, thereby synergistically exerting an excellent water blocking and anti-seepage effect to obtain component A;
[0020] S2. Add 10.0-15.0 g of oxalic acid to 50 mL of ethylene glycol solution and mix well to form a curing solvent. Oxalic acid catalyzes the curing reaction of the epoxy resin and shortens the curing time. Ethylene glycol can improve the viscosity of the resin, making it more uniform during the curing process and avoiding local uneven curing. It can also react with the ester bond of the epoxy resin to improve the molecular structure to obtain component B.
[0021] S3, mixing component A and component B evenly, component B can not only act as a curing agent, but also increase the toughness and impact resistance of the polymer and improve the mechanical properties, to obtain a new sol resin slurry;
[0022] Preferably, in step S1, the surfactant is an acetylene glycol surfactant, which can improve the wetting and permeability of the epoxy resin slurry, and is conducive to penetrating into cracks and concrete pore structures to achieve solidification and leak plugging.
[0023] The beneficial effects achieved by the present invention are as follows:
[0024] The present invention effectively improves the toughness and impact resistance of epoxy resin by adding core-shell nano-modified microspheres and composite super absorbent resin to the epoxy resin slurry of component A, and then mixes it with component B to improve the durability of the sol resin slurry after curing, and significantly enhances the water blocking and anti-seepage effect; in the core-shell nano-modified microspheres, the combination of inorganic materials and organic polymers forms core-shell structured microspheres that take into account both flexibility and rigidity, wherein the flexible shell absorbs water and swells, and is retained by adsorption, capture, bridging, etc., and the rigid core is blocked in the pores. The synergistic effect of the two effectively blocks the flow of water, and the microsphere structure also has good stability and durability, and can break through and advance under pressure, further enhancing the water blocking and anti-seepage effect; in the composite super absorbent resin, a quaternary composite cross-linked network structure is formed, which has excellent water absorption and swelling and adhesion, and can fill cracks and pores by absorbing water to swell the volume, and can also adhere to the area around the cracks to reduce water. The loss and movement caused by scouring can ensure a long-lasting and stable water-blocking and anti-seepage effect; the core-shell nano-modified microspheres can improve the pressure-bearing capacity of the composite super absorbent resin, and the composite super absorbent resin also optimizes the specific surface area of the core-shell nano-modified microspheres, thereby improving the water absorption performance of the microspheres. The core-shell nano-modified microspheres and the composite super absorbent resin are dispersed in the epoxy resin slurry, so that the microsphere structure and the resin network structure are better interspersed and distributed, effectively improving the toughness and impact resistance of the epoxy resin, reducing cracking and falling off after curing, and the B component curing solvent further reacts with the ester bond of the epoxy resin, which not only improves the curing uniformity of the component substances, but also improves the molecular structure of the epoxy resin, further improves the toughness and impact resistance, and is conducive to the continuous and effective play of water-blocking and anti-seepage effects; the present invention uses component A and component B to prepare a new type of sol resin slurry, which improves the toughness and impact resistance of the epoxy resin, enhances the durability of the slurry material, and achieves excellent water-blocking and anti-seepage effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope image of the core-shell nano-modified microspheres prepared in Example 1 of the present invention;
[0026] Figure 2 This is a scanning electron microscope image of the composite superabsorbent resin prepared in Example 1 of the present invention;
[0027] Figure 3 The figures are the mechanical properties results of Examples 1-4 and Comparative Examples 1-3 of the present invention;
[0028] Figure 4 This is a graph showing the water blocking rate results of Examples 1-4 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those familiar to those skilled in the art. Furthermore, any methods and materials similar or equivalent to those described herein can be applied to the present invention. The preferred embodiments and materials described herein are for illustrative purposes only and are not intended to limit the scope of this application.
[0031] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0032] The sources of the reagents used in the examples are as follows:
[0033] Silicon dioxide CAS No: 60676-86-0, brand Innochem, product number A98549;
[0034] KH-570 brand Xuanhao New Materials, item number KH-570;
[0035] Hydrochloric acid CAS No: 7647-01-0, brand Innochem, product number A04558;
[0036] Siban 80 CAS No: 1338-43-8, brand Innochem, product number A04343;
[0037] Tween 60 CAS No: 9005-67-8, brand Innochem, product number A78555;
[0038] Liquid paraffin CAS No: 8012-95-1, brand Acros, product number 171400010;
[0039] Acrylic acid CAS No: 79-10-7, brand Innochem, product number A24881;
[0040] Acrylamide CAS No: 79-06-1, brand Innochem, product number A26589;
[0041] 2-Acrylamido-2-methylpropanesulfonic acid CAS No: 15214-89-8, brand Innochem, product number A08586;
[0042] N,N-methylenebisacrylamide CAS No: 110-26-9, brand Innochem, product number A16528;
[0043] Sodium bicarbonate CAS No: 144-55-8, brand Innochem, product number A55543;
[0044] Ammonium persulfate CAS No: 7727-54-0, brand Innochem, product number A68367;
[0045] Sodium bisulfite CAS No: 7631-90-5, brand Innochem, product number A55110;
[0046] Montmorillonite CAS No: 1318-93-0, brand Innochem, product number A77948;
[0047] Octadecyltrimethylammonium bromide CAS No: 1120-02-1, brand Innochem, product number A95144;
[0048] 3-Aminopropyltriethoxysilane CAS No: 3663-44-3, brand Innochem, product number A04604;
[0049] Starch CAS No: 9005-25-8, brand Acros, product number 419695000;
[0050] Potassium persulfate CAS No: 7727-21-1, brand Innochem, product number A76563;
[0051] Epoxy resin CAS No: 38891-59-7, brand Fusion, product number FZ-0151577-100g;
[0052] Butyl glycidyl ether CAS No: 2426-08-6, brand Tci, product number B0697;
[0053] Oxalic acid CAS No: 144-62-7, brand Innochem, product number A18284;
[0054] Ethylene glycol CAS No: 107-21-1, brand Innochem, product number A82640;
[0055] Alkyne diol surfactant CAS No: 9014-85-1, brand Shanghai Canghong, item number 604;
[0056] Sodium hydroxide CAS No: 1310-73-2, brand Innochem, product number A36865;
[0057] Anhydrous ethanol CAS No: 64-17-5, brand Innochem, product number G00004.
[0058] Example 1
[0059] This embodiment proposes a novel sol resin slurry, comprising the following components in parts by weight: 90 parts of component A and 30 parts of component B.
[0060] Component A comprises the following components in parts by weight: 100 parts of epoxy resin slurry, 20 parts of core-shell nano-modified microspheres, 20 parts of composite super absorbent resin, and 8 parts of surfactant.
[0061] Component B is a solidifying solvent formed by dissolving oxalic acid in ethylene glycol solution.
[0062] The preparation method of core-shell nano-modified microspheres specifically comprises the following steps:
[0063] (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 100 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a hydrochloric acid solution with a mass fraction of 10.0%, ultrasonicate for 45 minutes, heat to 50 ° C, react for 2 hours, centrifuge to obtain a precipitate, and wash it with anhydrous ethanol 5 times, and vacuum dry. KH-570 forms an organic adsorption layer on the surface of the silica particles through its hydrolyzed group, which improves the dispersibility and stability of silica, and can also improve the disadvantage of silica being brittle at low temperatures, thereby obtaining modified silica;
[0064] (2) Add 0.7g of Span 80 and 0.2g of Tween 60 to 30.0g of liquid paraffin, stir until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0g of acrylic acid, 4.0g of acrylamide, 0.55g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015g of N,N-methylenebisacrylamide to 20.0g of water. The amount of modified silica added is 0.8g. When impacted, the modified silica can absorb part of the energy and reduce the generation and expansion of cracks, thereby enhancing the mechanical properties and compatibility of the microspheres and cooperating with the microspheres to improve the impact resistance and toughness of the epoxy resin. After stirring until completely dissolved, adjust the pH to 7.0 with a 5.0% sodium bicarbonate solution by mass, and use as the water phase. At 50°C, add 0.0 0.08g ammonium persulfate and 0.008g sodium bisulfite were dissolved in 2mL distilled water and then added dropwise to a three-necked flask. The oil phase and the aqueous phase were mixed, stirred evenly and poured into the flask. Nitrogen was passed through for deoxygenation. After stirring for 15min, the reaction was continued for 4h. The crude product was obtained by demulsification, filtration and centrifugation, and washed with anhydrous ethanol 5 times and vacuum dried. The modified nano-microspheres prepared by this method have a special core-shell structure. The polymer flexible shell on the surface of the microspheres absorbs water and swells, and is retained by adsorption, capture, bridging, etc. The rigid core is blocked in the pores. The synergistic effect of the two effectively prevents the flow of water and achieves the purpose of water blocking and anti-seepage. The microsphere structure also has good stability and durability, can exist stably in water, and can break through and advance under pressure, which further enhances the effect of water blocking and anti-seepage, and obtains core-shell nano-modified microspheres.
[0065] The preparation method of the composite super absorbent resin specifically comprises the following steps:
[0066] a. Add 1.0 g of montmorillonite to 100 mL of water, stir at 300 rpm for 12 h, then place it in an ultrasonic cell disruptor and ultrasonicate it at 450 W for 5 min. The multilayer montmorillonite is mechanically exfoliated into a low-dimensional structure by ultrasonic treatment, which has a large specific surface area and abundant active sites. Then, 0.1 g of octadecyltrimethylammonium bromide is added, and the amount of octadecyltrimethylammonium bromide added is 1.0 g. The octadecyltrimethylammonium bromide achieves the effect of fully hydrating and dispersing the montmorillonite through chemical exfoliation, further reducing the dimension of the montmorillonite structure. Stir at 50 ° C for 5 h, wash the reduced-dimensional montmorillonite with anhydrous ethanol, add it to 200 mL of water and stir. The mechanical and chemical exfoliation treatment method effectively destroys the multilayer structure of montmorillonite and decomposes it into a low-dimensional or even single-layer lamellar structure, which can be used for nano-blocking materials to obtain a nano-montmorillonite suspension.
[0067] b. 0.2 mL of a 2.0% aqueous solution of 3-aminopropyltriethoxysilane by mass was added dropwise to the nano-montmorillonite suspension described in step a at a constant temperature of 50° C. and stirred for 24 hours. After the reaction was completed, the suspension was centrifuged at a speed of 5000 rpm for 5 minutes, and the precipitate was washed 5 times with anhydrous ethanol and dried in vacuo. The montmorillonite after amination treatment further enhanced the adsorption capacity and stability of the montmorillonite by introducing amino groups, effectively absorbed and fixed water, reduced the flow and penetration of the liquid, and had excellent water blocking and anti-seepage effects, thereby obtaining aminated montmorillonite;
[0068] c. 8.0g starch and 2.0g amination montmorillonite described in step b were added to 50mL water and gelatinized at a constant temperature of 60°C for 1h. Stand-by, then 5.0g acrylic acid was weighed in a conical flask filled with 20mL distilled water, and 20mL of sodium hydroxide solution with a mass fraction of 10% was added dropwise under ice-water bath conditions. After neutralization, 1.0g 2-acrylamide-2-methylpropanesulfonic acid was added and stirred evenly. It was used as a monomer for stand-by. 0.7g of Span 80 and 0.2g of Tween 60 were added to 30.0g of liquid paraffin, and mechanically stirred at a constant temperature of 55°C for 1h. After forming a stable oil phase, starch and amination montmorillonite solution were slowly added to the oil phase, emulsified at 55°C for 1h, and finally monomers, 2.0g of potassium persulfate and 0.04g of N, N-methylenebisacrylamide were added in sequence. The ultrasonic instrument is used for degassing treatment, which can prevent the formation of large pore structures and is conducive to the formation of uniform pore structures, thereby showing good elasticity and strength, improving the toughness and impact resistance of the resin, and improving its durability. The reaction is then stirred at 55°C for 3 hours, the product is cooled to room temperature, and washed with distilled water 5 times, vacuum filtered, dried, and crushed. The composite resin prepared with starch and modified montmorillonite as raw materials, vinyl monomer and acrylic acid has high water absorption and swelling properties and excellent adhesion. When used in cracks and penetration areas, it will adhere to the surrounding building materials, absorb overflowing water, cause its own volume to expand, and thus fill cracks and pores. Its excellent adhesion ability effectively reduces the scouring of water flow or other factors, reduces loss or movement, enhances the sealing effect, and obtains a composite superabsorbent resin.
[0069] This embodiment provides a method for preparing a novel sol resin slurry, which specifically includes the following steps:
[0070] S1, 100g epoxy resin is dissolved in 10mL butyl glycidyl ether, epoxy resin slurry is formed, then core-shell nano modified microspheres, composite super absorbent resin and surfactant are added thereto, surfactant is acetylene glycol surfactant, acetylene glycol surfactant can improve the wetting and permeability of epoxy resin slurry, is conducive to realizing solidification plugging in deep crack and concrete pore structure, stir evenly, core-shell nano modified microspheres and composite super absorbent resin have good compatibility, can be evenly dispersed in epoxy resin slurry, again because of the adding of spherical structure and composite resin cross-linked network structure, improve the toughness and impact property of epoxy resin, enhance water absorption and swelling ability, wherein, core-shell nano modified microspheres make up the bearing capacity of composite super absorbent resin, and composite super absorbent resin further enhances the water absorption and stability of core-shell nano modified microspheres, thus synergistically play excellent water blocking and anti-seepage effect, obtain A component;
[0071] S2. Add 15.0 g of oxalic acid to 50 mL of ethylene glycol solution and mix well to form a curing solvent. Oxalic acid catalyzes the curing reaction of the epoxy resin and shortens the curing time. Ethylene glycol can improve the viscosity of the resin, making it more uniform during the curing process and avoiding local uneven curing. It can also react with the ester bond of the epoxy resin to improve the molecular structure to obtain component B.
[0072] S3. Component A and component B are mixed evenly. Component B can act as a curing agent and increase the toughness and impact resistance of the polymer, thereby improving mechanical properties to obtain a new sol resin slurry.
[0073] In this example, the prepared core-shell nano-modified microspheres and composite super absorbent resin were subjected to scanning electron microscopy to observe their microscopic morphology. Figure 1 This is a 100,000-fold magnified SEM image of the core-shell nano-modified microspheres prepared in Example 1. Figure 2 This is a 400-fold magnified SEM image of the composite super absorbent resin prepared in Example 1. Figure 1 The core-shell nano-modified microspheres prepared in this embodiment present a core-shell spherical structure, as shown in FIG. Figure 2 The composite super absorbent resin prepared in this embodiment has a dense cross-linked network structure.
[0074] Example 2
[0075] This embodiment proposes a novel sol resin slurry, comprising the following components in parts by weight: 60 parts of component A and 20 parts of component B.
[0076] Component A comprises the following components in parts by weight: 80 parts of epoxy resin slurry, 10 parts of core-shell nano-modified microspheres, 10 parts of composite superabsorbent resin, and 5 parts of surfactant.
[0077] Component B is a solidifying solvent formed by dissolving oxalic acid in ethylene glycol solution.
[0078] The preparation method of core-shell nano-modified microspheres specifically comprises the following steps:
[0079] (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 50 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a 5.0% hydrochloric acid solution. Ultrasonicate for 25 min, heat to 40 ° C, react for 1 h, centrifuge to obtain a precipitate, and wash it with anhydrous ethanol three times, and vacuum dry. KH-570 forms an organic adsorption layer on the surface of the silica particles through its hydrolyzed group, which improves the dispersibility and stability of silica, and can also improve the disadvantage of silica being brittle at low temperatures, thereby obtaining modified silica;
[0080] (2) Add 0.7g of Span 80 and 0.2g of Tween 60 to 30.0g of liquid paraffin, stir until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0g of acrylic acid, 4.0g of acrylamide, 0.55g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015g of N,N-methylenebisacrylamide to 20.0g of water. The amount of modified silica added is 0.7g. When impacted, the modified silica can absorb part of the energy and reduce the generation and expansion of cracks, thereby enhancing the mechanical properties and compatibility of the microspheres and cooperating with the microspheres to improve the impact resistance and toughness of the epoxy resin. After stirring until completely dissolved, adjust the pH to 7.0 with a 5.0% sodium bicarbonate solution by mass, and use as the water phase. At 40°C, add 0.00 8g of ammonium persulfate and 0.008g of sodium bisulfite are dissolved in 1-2mL of distilled water, and then added dropwise to a three-necked flask. The oil phase and the aqueous phase are mixed, stirred evenly, and then poured into the flask. Nitrogen is passed through for deoxygenation, and the reaction is continued for 3h after stirring for 10min. The crude product is obtained by demulsification, filtration, and centrifugation, and is washed with anhydrous ethanol 3 times and vacuum dried. The modified nano-microspheres prepared by this method have a special core-shell structure. The polymer flexible shell on the surface of the microsphere absorbs water and swells, and is retained by adsorption, capture, bridging, etc. The rigid core is blocked in the pores. The synergistic effect of the two effectively prevents the flow of water and achieves the purpose of water blocking and anti-seepage. The microsphere structure also has good stability and durability, can exist stably in water, and can break through and advance under pressure, thereby further enhancing the effect of water blocking and anti-seepage, and obtaining core-shell nano-modified microspheres.
[0081] The preparation method of the composite super absorbent resin specifically comprises the following steps:
[0082] a. Add 1.0 g of montmorillonite to 100 mL of water, stir at 100 rpm for 8 h, then place it in an ultrasonic cell disruptor and ultrasonicate it at 350 W for 3 min. The multilayer montmorillonite is mechanically exfoliated into a low-dimensional structure with a large specific surface area and abundant active sites by ultrasonic treatment. Then, 0.1 g of octadecyltrimethylammonium bromide is added, and the amount of octadecyltrimethylammonium bromide added is 1.0 g. The octadecyltrimethylammonium bromide achieves the effect of fully hydrating and dispersing the montmorillonite through chemical exfoliation, further reducing the dimension of the montmorillonite structure. Stir at 40 ° C for 3 h, wash the reduced-dimensional montmorillonite with anhydrous ethanol, add it to 200 mL of water and stir. The mechanical and chemical synergistic exfoliation treatment method effectively destroys the multilayer structure of montmorillonite and decomposes it into a low-dimensional or even single-layer lamellar structure, which can be used for nano-blocking materials to obtain a nano-montmorillonite suspension.
[0083] b. 0.2 mL of a 1.0% aqueous solution of 3-aminopropyltriethoxysilane by mass was added dropwise to the nano-montmorillonite suspension described in step a at a constant temperature of 50° C. and stirred for 24 hours. After the reaction was completed, the suspension was centrifuged at a speed of 5000 rpm for 3 minutes, and the precipitate was washed 3 times with anhydrous ethanol and dried in vacuo. The montmorillonite after amination treatment further enhanced the adsorption capacity and stability of the montmorillonite by introducing amino groups, effectively absorbed and fixed water, reduced the flow and penetration of the liquid, and had excellent water blocking and anti-seepage effects, thereby obtaining aminated montmorillonite;
[0084] c. 8.0g starch and 2.0g amination montmorillonite described in step b were added to 50mL water and gelatinized at a constant temperature of 50°C for 0.5h. Stand-by, 5.0g acrylic acid was weighed in a conical flask filled with 20mL distilled water, and 10mL of sodium hydroxide solution with a mass fraction of 10% was added dropwise under ice-water bath conditions. After neutralization, 1.0g 2-acrylamide-2-methylpropanesulfonic acid was added and stirred evenly. The mixture was used as a monomer. 0.7g of Span 80 and 0.2g of Tween 60 were added to 30.0g of liquid paraffin. The mixture was mechanically stirred at a constant temperature of 45°C for 0.5h. After forming a stable oil phase, the starch and amination montmorillonite solution were slowly added to the oil phase, emulsified at 45°C for 0.5h. Finally, monomers, 2.0g of potassium persulfate and 0.04g of N,N-methylenebisacrylamide were added in sequence. First, use an ultrasonic device for degassing treatment. Degassing treatment can prevent the formation of large pore structures and is conducive to the formation of uniform pore structures, thereby showing good elasticity and strength, improving the toughness and impact resistance of the resin, and improving its durability. Then, stir the reaction at 45°C for 2 hours, cool the product to room temperature, and wash it with distilled water 3 times, vacuum filter, dry, and crush. The composite resin prepared with starch and modified montmorillonite as raw materials, vinyl monomer and acrylic acid has high water absorption and swelling properties and excellent adhesion. When used in cracks and penetration areas, it will adhere to the surrounding building materials, absorb overflowing water, cause its own volume to expand, and thus fill cracks and pores. Its excellent adhesion ability effectively reduces the scouring of water flow or other factors, reduces loss or movement, enhances the sealing effect, and obtains a composite superabsorbent resin.
[0085] This embodiment provides a method for preparing a novel sol resin slurry, which specifically includes the following steps:
[0086] S1, 100g epoxy resin is dissolved in 10mL butyl glycidyl ether, epoxy resin slurry is formed, then core-shell nano modified microspheres, composite super absorbent resin and surfactant are added thereto, surfactant is acetylene glycol surfactant, acetylene glycol surfactant can improve the wetting and permeability of epoxy resin slurry, is conducive to realizing solidification plugging in deep crack and concrete pore structure, stir evenly, core-shell nano modified microspheres and composite super absorbent resin have good compatibility, can be evenly dispersed in epoxy resin slurry, again because of the adding of spherical structure and composite resin cross-linked network structure, improve the toughness and impact property of epoxy resin, enhance water absorption and swelling ability, wherein, core-shell nano modified microspheres make up the bearing capacity of composite super absorbent resin, and composite super absorbent resin further enhances the water absorption and stability of core-shell nano modified microspheres, thus synergistically play excellent water blocking and anti-seepage effect, obtain A component;
[0087] S2. Add 10.0 g of oxalic acid to 50 mL of ethylene glycol solution and mix well to form a curing solvent. Oxalic acid catalyzes the curing reaction of the epoxy resin and shortens the curing time. Ethylene glycol can improve the viscosity of the resin, making it more uniform during the curing process and avoiding local uneven curing. It can also react with the ester bond of the epoxy resin to improve the molecular structure to obtain component B.
[0088] S3. Component A and component B are mixed evenly. Component B can act as a curing agent and increase the toughness and impact resistance of the polymer, thereby improving mechanical properties to obtain a new sol resin slurry.
[0089] Example 3
[0090] This embodiment proposes a novel sol resin slurry, comprising the following components in parts by weight: 75 parts of component A and 25 parts of component B.
[0091] Component A comprises the following components in parts by weight: 90 parts of epoxy resin slurry, 15 parts of core-shell nano-modified microspheres, 15 parts of composite superabsorbent resin, and 6.5 parts of surfactant.
[0092] Component B is a solidifying solvent formed by dissolving oxalic acid in ethylene glycol solution.
[0093] The preparation method of core-shell nano-modified microspheres specifically comprises the following steps:
[0094] (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 75 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a 7.5% hydrochloric acid solution. Ultrasonicate for 35 min, heat to 45 ° C, react for 1.5 h, centrifuge to obtain a precipitate, and wash it with anhydrous ethanol 4 times, and vacuum dry. KH-570 forms an organic adsorption layer on the surface of the silica particles through its hydrolyzed group, which improves the dispersibility and stability of silica, and can also improve the disadvantage of silica being brittle at low temperatures, thereby obtaining modified silica;
[0095] (2) Add 0.7g of Span 80 and 0.2g of Tween 60 to 30.0g of liquid paraffin, stir until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0g of acrylic acid, 4.0g of acrylamide, 0.55g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015g of N,N-methylenebisacrylamide to 20.0g of water. The amount of modified silica added is 0.75g. When impacted, the modified silica can absorb part of the energy and reduce the generation and expansion of cracks, thereby enhancing the mechanical properties and compatibility of the microspheres and cooperating with the microspheres to improve the impact resistance and toughness of the epoxy resin. After stirring until completely dissolved, adjust the pH to 7.0 with a 5.0% sodium bicarbonate solution by mass, and use as the water phase. At 45°C, add 0.008g of Ammonium persulfate and 0.008g sodium bisulfite were dissolved in 1.5mL distilled water and then added dropwise to a three-necked flask. The oil phase and the aqueous phase were mixed, stirred evenly, and poured into the flask. Nitrogen was passed through for deoxygenation, and the reaction was continued for 3.5h after stirring for 12.5min. The crude product was obtained by demulsification, filtration, and centrifugation, and washed with anhydrous ethanol 4 times and vacuum dried. The modified nano-microspheres prepared by this method have a special core-shell structure. The polymer flexible shell on the surface of the microspheres absorbs water and swells, and is retained by adsorption, capture, bridging, etc. The rigid core is blocked in the pores. The synergistic effect of the two effectively prevents the flow of water and achieves the purpose of water blocking and anti-seepage. The microsphere structure also has good stability and durability, can exist stably in water, and can break through and advance under pressure, thereby further enhancing the effect of water blocking and anti-seepage, and obtaining core-shell nano-modified microspheres.
[0096] The preparation method of the composite super absorbent resin specifically comprises the following steps:
[0097] a. Add 1.0 g of montmorillonite to 100 mL of water, stir at 200 rpm for 10 h, then place it in an ultrasonic cell disruptor and ultrasonicate it at 400 W for 4 min. The multilayer montmorillonite is mechanically exfoliated into a low-dimensional structure by ultrasonic treatment, which has a large specific surface area and abundant active sites. Then, 0.1 g of octadecyltrimethylammonium bromide is added, and the amount of octadecyltrimethylammonium bromide added is 1.0 g. The octadecyltrimethylammonium bromide achieves the effect of fully hydrating and dispersing the montmorillonite through chemical exfoliation, further reducing the dimension of the montmorillonite structure. Stir at 45 ° C for 4 h, wash the reduced-dimensional montmorillonite with anhydrous ethanol, add it to 200 mL of water and stir. The mechanical and chemical exfoliation treatment method effectively destroys the multilayer structure of montmorillonite and decomposes it into a low-dimensional or even single-layer lamellar structure, which can be used for nano-blocking materials to obtain a nano-montmorillonite suspension.
[0098] b. 0.2 mL of a 1.5% mass fraction of 3-aminopropyltriethoxysilane aqueous solution was added dropwise to the nano-montmorillonite suspension described in step a at a constant temperature of 50° C. and stirred for 24 hours. After the reaction, the solution was centrifuged at 5000 rpm for 4 minutes, and the precipitate was washed 4 times with anhydrous ethanol and dried in vacuo. The montmorillonite after amination treatment further enhanced the adsorption capacity and stability of the montmorillonite by introducing amino groups, effectively absorbed and fixed water, reduced the flow and penetration of the liquid, and had excellent water blocking and anti-seepage effects, thereby obtaining aminated montmorillonite;
[0099] c. 8.0g starch and 2.0g amination montmorillonite described in step b were added to 50mL water and gelatinized at a constant temperature of 55°C for 0.8h. Stand-by, 5.0g acrylic acid was weighed in a conical flask filled with 20mL distilled water, and 15mL of sodium hydroxide solution with a mass fraction of 10% was added dropwise under ice-water bath conditions. After neutralization, 1.0g 2-acrylamide-2-methylpropanesulfonic acid was added and stirred evenly. It was used as a monomer for stand-by. 0.7g of Span 80 and 0.2g of Tween 60 were added to 30.0g of liquid paraffin, and mechanically stirred at a constant temperature of 50°C for 0.8h. After forming a stable oil phase, starch and amination montmorillonite solution were slowly added to the oil phase, emulsified at 50°C for 0.8h, and finally monomers, 2.0g of potassium persulfate and 0.04g of N, N-methylenebisacrylamide were added in sequence. An ultrasonic device is used for degassing treatment, which can prevent the formation of large pore structures and is conducive to the formation of uniform pore structures, thereby showing good elasticity and strength, improving the toughness and impact resistance of the resin, and improving its durability. The reaction is then stirred at 50°C for 2.5 hours, the product is cooled to room temperature, and washed with distilled water 4 times, vacuum filtered, dried, and crushed. The composite resin prepared with starch and modified montmorillonite as raw materials, vinyl monomer and acrylic acid has high water absorption and swelling properties and excellent adhesion. When used in cracks and penetration areas, it will adhere to the surrounding building materials, absorb overflowing water, cause its own volume to expand, and thus fill cracks and pores. Its excellent adhesion ability effectively reduces the scouring of water flow or other factors, reduces loss or movement, enhances the sealing effect, and obtains a composite superabsorbent resin.
[0100] This embodiment provides a method for preparing a novel sol resin slurry, which specifically includes the following steps:
[0101] S1, 100g epoxy resin is dissolved in 10mL butyl glycidyl ether, epoxy resin slurry is formed, then core-shell nano modified microspheres, composite super absorbent resin and surfactant are added thereto, surfactant is acetylene glycol surfactant, acetylene glycol surfactant can improve the wetting and permeability of epoxy resin slurry, is conducive to realizing solidification plugging in deep crack and concrete pore structure, stir evenly, core-shell nano modified microspheres and composite super absorbent resin have good compatibility, can be evenly dispersed in epoxy resin slurry, again because of the adding of spherical structure and composite resin cross-linked network structure, improve the toughness and impact property of epoxy resin, enhance water absorption and swelling ability, wherein, core-shell nano modified microspheres make up the bearing capacity of composite super absorbent resin, and composite super absorbent resin further enhances the water absorption and stability of core-shell nano modified microspheres, thus synergistically play excellent water blocking and anti-seepage effect, obtain A component;
[0102] S2. Add 12.5 g of oxalic acid to 50 mL of ethylene glycol solution and mix well to form a curing solvent. Oxalic acid catalyzes the curing reaction of the epoxy resin and shortens the curing time. Ethylene glycol can improve the viscosity of the resin, making it more uniform during the curing process and avoiding local uneven curing. It can also react with the ester bond of the epoxy resin to improve the molecular structure to obtain component B.
[0103] S3. Component A and component B are mixed evenly. Component B can act as a curing agent and increase the toughness and impact resistance of the polymer, thereby improving mechanical properties to obtain a new sol resin slurry.
[0104] Example 4
[0105] This embodiment proposes a novel sol resin slurry, comprising the following components in parts by weight: 60 parts of component A and 30 parts of component B.
[0106] Component A comprises the following components in parts by weight: 100 parts of epoxy resin slurry, 10 parts of core-shell nano-modified microspheres, 20 parts of composite superabsorbent resin, and 8 parts of surfactant.
[0107] Component B is a solidifying solvent formed by dissolving oxalic acid in ethylene glycol solution.
[0108] The preparation method of core-shell nano-modified microspheres specifically comprises the following steps:
[0109] (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 100 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a hydrochloric acid solution with a mass fraction of 10.0%, ultrasonicate for 25 minutes, heat to 50 ° C, react for 1 hour, centrifuge to obtain a precipitate, and wash it with anhydrous ethanol 5 times, and vacuum dry. KH-570 forms an organic adsorption layer on the surface of the silica particles through its hydrolyzed group, which improves the dispersibility and stability of silica, and can also improve the disadvantage of silica being brittle at low temperatures, thereby obtaining modified silica;
[0110] (2) Add 0.7g of Span 80 and 0.2g of Tween 60 to 30.0g of liquid paraffin, stir until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0g of acrylic acid, 4.0g of acrylamide, 0.55g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015g of N,N-methylenebisacrylamide to 20.0g of water. The amount of modified silica added is 0.8g. When impacted, the modified silica can absorb part of the energy and reduce the generation and expansion of cracks, thereby enhancing the mechanical properties and compatibility of the microspheres and cooperating with the microspheres to improve the impact resistance and toughness of the epoxy resin. After stirring until completely dissolved, adjust the pH to 7.0 with a 5.0% sodium bicarbonate solution by mass, and use as the water phase. At 50°C, add 0.0 0.08g ammonium persulfate and 0.008g sodium bisulfite were dissolved in 2mL distilled water and then added dropwise to a three-necked flask. The oil phase and the aqueous phase were mixed, stirred evenly and poured into the flask. Nitrogen was passed through for deoxygenation and the reaction was continued for 3h after stirring for 10min. The crude product was obtained by demulsification, filtration and centrifugation, and washed with anhydrous ethanol 5 times and vacuum dried. The modified nano-microspheres prepared by this method have a special core-shell structure. The polymer flexible shell on the surface of the microspheres absorbs water and swells, and is retained by adsorption, capture, bridging and the like. The rigid core is blocked in the pores. The synergistic effect of the two effectively prevents the flow of water and achieves the purpose of water blocking and anti-seepage. The microsphere structure also has good stability and durability, can exist stably in water, and can break through and advance under pressure, thereby enhancing the effect of water blocking and anti-seepage, and obtaining core-shell nano-modified microspheres.
[0111] The preparation method of the composite super absorbent resin specifically comprises the following steps:
[0112] a. Add 1.0 g of montmorillonite to 100 mL of water, stir at 300 rpm for 8 h, then place it in an ultrasonic cell disruptor and ultrasonicate it at 450 W for 3 min. The multilayer montmorillonite is mechanically exfoliated into a low-dimensional structure by ultrasonic treatment, which has a large specific surface area and abundant active sites. Then, 0.1 g of octadecyltrimethylammonium bromide is added, and the amount of octadecyltrimethylammonium bromide added is 1.0 g. The octadecyltrimethylammonium bromide achieves the effect of fully hydrating and dispersing the montmorillonite through chemical exfoliation, further reducing the dimension of the montmorillonite structure. Stir at 50 ° C for 3 h, wash the reduced-dimensional montmorillonite with anhydrous ethanol, add it to 200 mL of water and stir. The mechanical and chemical synergistic exfoliation treatment method effectively destroys the multilayer structure of montmorillonite and decomposes it into a low-dimensional or even single-layer lamellar structure, which can be used for nano-blocking materials to obtain a nano-montmorillonite suspension.
[0113] b. 0.2 mL of a 2.0% aqueous solution of 3-aminopropyltriethoxysilane by mass was added dropwise to the nano-montmorillonite suspension described in step a at a constant temperature of 50° C. and stirred for 24 hours. After the reaction was completed, the mixture was centrifuged at a speed of 5000 rpm for 3 minutes, and the precipitate was washed 5 times with anhydrous ethanol and dried in vacuo. The montmorillonite after amination treatment further enhanced the adsorption capacity and stability of the montmorillonite by introducing amino groups, effectively absorbed and fixed water, reduced the flow and penetration of the liquid, and had excellent water blocking and anti-seepage effects, thereby obtaining aminated montmorillonite;
[0114] c. 8.0g starch and 2.0g amination montmorillonite described in step b were added to 50mL water and gelatinized at a constant temperature of 60°C for 0.5h. Stand-by, 5.0g acrylic acid was weighed in a conical flask filled with 20mL distilled water, and 20mL of sodium hydroxide solution with a mass fraction of 10% was added dropwise under ice-water bath conditions. After neutralization, 1.0g 2-acrylamide-2-methylpropanesulfonic acid was added and stirred evenly. The mixture was used as a monomer. 0.7g of Span 80 and 0.2g of Tween 60 were added to 30.0g of liquid paraffin. The mixture was mechanically stirred at a constant temperature of 55°C for 0.5h. After forming a stable oil phase, the starch and amination montmorillonite solution were slowly added to the oil phase, emulsified at 55°C for 0.5h. Finally, monomers, 2.0g of potassium persulfate and 0.04g of N,N-methylenebisacrylamide were added in sequence. First, use an ultrasonic device for degassing treatment. Degassing treatment can prevent the formation of large pore structures and is conducive to the formation of uniform pore structures, thereby showing good elasticity and strength, improving the toughness and impact resistance of the resin, and improving its durability. Then, stir the reaction at 55°C for 2 hours, cool the product to room temperature, and wash it with distilled water 5 times, vacuum filter, dry, and crush. The composite resin prepared with starch and modified montmorillonite as raw materials, vinyl monomer and acrylic acid has high water absorption and swelling properties and excellent adhesion. When used in cracks and penetration areas, it will adhere to the surrounding building materials, absorb overflowing water, cause its own volume to expand, and thus fill cracks and pores. Its excellent adhesion ability effectively reduces the scouring of water flow or other factors, reduces loss or movement, enhances the sealing effect, and obtains a composite superabsorbent resin.
[0115] This embodiment provides a method for preparing a novel sol resin slurry, which specifically includes the following steps:
[0116] S1, 100g epoxy resin is dissolved in 10mL butyl glycidyl ether, epoxy resin slurry is formed, then core-shell nano modified microspheres, composite super absorbent resin and surfactant are added thereto, surfactant is acetylene glycol surfactant, acetylene glycol surfactant can improve the wetting and permeability of epoxy resin slurry, is conducive to realizing solidification plugging in deep crack and concrete pore structure, stir evenly, core-shell nano modified microspheres and composite super absorbent resin have good compatibility, can be evenly dispersed in epoxy resin slurry, again because of the adding of spherical structure and composite resin cross-linked network structure, improve the toughness and impact property of epoxy resin, enhance water absorption and swelling ability, wherein, core-shell nano modified microspheres make up the bearing capacity of composite super absorbent resin, and composite super absorbent resin further enhances the water absorption and stability of core-shell nano modified microspheres, thus synergistically play excellent water blocking and anti-seepage effect, obtain A component;
[0117] S2. Add 15.0 g of oxalic acid to 50 mL of ethylene glycol solution and mix well to form a curing solvent. Oxalic acid catalyzes the curing reaction of the epoxy resin and shortens the curing time. Ethylene glycol can improve the viscosity of the resin, making it more uniform during the curing process and avoiding local uneven curing. It can also react with the ester bond of the epoxy resin to improve the molecular structure to obtain component B.
[0118] S3. Component A and component B are mixed evenly. Component B can act as a curing agent and increase the toughness and impact resistance of the polymer, thereby improving mechanical properties to obtain a new sol resin slurry.
[0119] Comparative Example 1
[0120] This comparative example provides a novel sol resin slurry, which differs from Example 1 in that the core-shell nano-modified microspheres do not contain modified silica; the preparation method of the core-shell nano-modified microspheres does not include step (1); the preparation method of the composite superabsorbent resin is the same as that of Example 1; and the preparation method of the novel sol resin slurry is the same as that of Example 1.
[0121] Comparative Example 2
[0122] This comparative example provides a new sol resin slurry, which differs from Example 1 in that the composite superabsorbent resin does not contain amino montmorillonite; the preparation method of the core-shell nano-modified microspheres is the same as that of Example 1; the preparation method of the composite superabsorbent resin does not include steps a and b; the preparation method of the new sol resin slurry is the same as that of Example 1.
[0123] Comparative Example 3
[0124] This comparative example provides a new sol resin slurry, which differs from Example 1 in that component B does not contain ethylene glycol; the preparation method of core-shell nano-modified microspheres is the same as that of Example 1; the preparation method of the composite superabsorbent resin is the same as that of Example 1; and the preparation method of the new sol resin slurry is the same as that of Example 1.
[0125] Experimental Example 1
[0126] Mechanical properties test
[0127] Test sample: the novel sol resin slurry prepared in Examples 1-4 and Comparative Examples 1-3.
[0128] Test method: (1) The tensile strength and elongation tests were carried out in accordance with GB / T2567-2021 standard. The test samples were solidified into specimens. During the test, the loading rate was controlled at 10 mm / min. Five specimens were tested in each group. The test results of tensile strength (MPa) and elongation (%) were averaged.
[0129] (2) Impact toughness test was carried out according to GB / T2567-2021 standard. The test samples were solidified and made into specimens. During the test, the speed of the pendulum impacting the center of the specimen was controlled to be 2.9m / s. Five specimens were tested in each group. The impact toughness (kJ·m -2 ) The test results are averaged.
[0130] Figure 3 The mechanical properties of Examples 1-4 and Comparative Examples 1-3 are shown in the figure. As shown in the figure, the tensile strength, elongation and impact toughness of Examples 1-4 are 73.1-78.2MPa, 33.2-36.5%, and 2.9-3.5kJ·m -2 , indicating good toughness and impact resistance; the tensile strength, elongation and impact toughness of Comparative Examples 1-3 were 56.5-64.8MPa, 23.7-28.9%, and 1.5-2.2kJ·m -2 , indicating that the toughness and impact resistance are poor; the core-shell nano-modified microspheres of Comparative Example 1 do not contain modified silica, which cannot absorb part of the energy to reduce the generation and expansion of cracks, nor can it form a spherical structure with a rigid core, which is not conducive to the improvement of the epoxy resin network structure, resulting in poor toughness and impact resistance; the composite super absorbent resin of Comparative Example 2 does not contain amino montmorillonite, which weakens the density of the composite resin network structure, which is not conducive to better interpenetration and filling of the epoxy resin structure, resulting in poor toughness and impact resistance; the new sol resin slurry of Comparative Example 3 does not contain ethylene glycol, which cannot react with the ester bond of the epoxy resin, is not conducive to improving the molecular structure of the epoxy resin, nor is it conducive to improving the curing uniformity of the various components, thereby adversely affecting the uniformity of the mechanical properties of the slurry after curing, resulting in poor toughness and impact resistance.
[0131] Experimental Example 2
[0132] Water blocking effect experiment
[0133] Test sample: the novel sol resin slurry prepared in Examples 1-4 and Comparative Examples 1-3.
[0134] Test method: A rough single crack grouting model was selected for the plugging test. The entire model is 1000mm x 500mm x 5mm in length, width and height. A groove with a width of 50mm and a depth of 10mm was left on each side of the model box. When water flows into the left end of the water inlet, the water first reaches the groove and then enters the rough crack, ensuring the stability of the water flow. First, use a stopwatch and a graduated cylinder to measure the initial water flow rate Q0 (cm 2 / s) is measured, and then the test sample is injected through the grouting hole. The slurry gradually reaches the edges of the model box and begins to solidify to form a blockage, blocking the flow of water. The water flow rate Q1 (cm 2 / s) and calculate the water blocking rate (%) according to the following formula:
[0135] Water blocking rate (%) = (Q0-Q1) / Q0×100%
[0136] Figure 4 The water blocking rate results of Examples 1-4 and Comparative Examples 1-3 are shown in the figure. As shown in the figure, the water blocking rate of Examples 1-4 is 90.2-92.4%, indicating that the water blocking and anti-seepage effect is better; the water blocking rate of Comparative Examples 1-3 is 78.5-85.7%, indicating that the water blocking and anti-seepage effect is not good; the core-shell nano-modified microspheres of Comparative Example 1 do not contain modified silica, and cannot form a rigid core structure and are blocked in the pores, which weakens the water blocking ability of the microspheres and is not conducive to improving the pressure bearing capacity of the composite super absorbent resin, limiting its stable performance. The water absorption and swelling effect results in poor water blocking and anti-seepage effect; the composite super absorbent resin of Comparative Example 2 does not contain amino montmorillonite, which reduces the ability of the composite super absorbent resin to absorb and fix water, is not conducive to reducing the flow and penetration of the liquid, and results in poor water blocking and anti-seepage effect; the new sol resin slurry of Comparative Example 3 does not contain ethylene glycol, which is not conducive to the solidification uniformity of the component substances, and thus is not conducive to the uniform and effective performance of the water blocking and anti-seepage effect of the core-shell nano-modified microspheres and the composite super absorbent resin, resulting in poor water blocking and anti-seepage effect.
[0137] The above experimental results show that the mechanical properties and water blocking effects of Examples 1-4 of the present invention are significantly better than those of Comparative Examples 1-3. Among them, Example 1 using core-shell nano-modified microspheres and composite super absorbent resin has better toughness and impact resistance and better water blocking effect. In the core-shell nano-modified microspheres, the flexible shell absorbs water and swells, and the rigid core blocks the pores. The synergistic effect of the two effectively blocks the flow of water. The composite super absorbent resin has excellent water absorption, swelling and adhesion. It can fill cracks and pores by absorbing water and swelling volume, and can also adhere to the cracks. Around the seam, it reduces the loss and movement caused by water scouring, ensuring a lasting and stable water blocking and anti-seepage effect. The core-shell nano-modified microspheres and composite super absorbent resin are dispersed in the epoxy resin slurry, so that the microsphere structure and the resin network structure are better interspersed and distributed, improving the toughness and impact resistance of the epoxy resin. In addition, the B component curing solvent further reacts with the ester bond of the epoxy resin, thereby improving the curing uniformity of the component substances, improving the molecular structure of the epoxy resin, and further improving the toughness and impact resistance, which is conducive to the continuous and effective play of the water blocking and anti-seepage effect.
[0138] While the embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions, and alterations can be made to the embodiments without departing from the principles and spirit of the invention.
[0139] The present invention and its embodiments are described above. Such description is not restrictive. The drawings show only one embodiment of the present invention, and actual applications are not limited thereto. In short, if a person skilled in the art is inspired by the above, and does not deviate from the purpose of the present invention, any method and embodiment similar to the technical solution without creative design shall fall within the scope of protection of the present invention.
Claims
1. A novel sol resin slurry, characterized in that: The novel sol resin slurry comprises the following components in parts by weight: 60-90 parts of component A and 20-30 parts of component B; the component A comprises the following components in parts by weight: 80-100 parts of epoxy resin slurry, 10-20 parts of core-shell nano-modified microspheres, 10-20 parts of composite highly absorbent resin, and 5-8 parts of surfactant; the component B is a curing solvent formed by dissolving oxalic acid in an ethylene glycol solution.
2. A method for preparing the novel sol resin slurry according to claim 1, characterized in that: The specific steps include: S1, dissolving 100g of epoxy resin in 10mL of butyl glycidyl ether to form an epoxy resin slurry, adding core-shell nano-modified microspheres, composite superabsorbent resin and surfactant thereto, stirring evenly to obtain component A; S2, adding 10.0-15.0 g of oxalic acid to 50 mL of ethylene glycol solution and mixing evenly to form a solidifying solvent to obtain component B; S3. Mix component A and component B evenly to obtain a novel sol resin slurry.
3. The method for preparing the novel sol resin slurry according to claim 2, characterized in that: In step S1, the surfactant is an acetylene glycol surfactant.
4. The method for preparing the novel sol resin slurry according to claim 3, characterized in that: The method for preparing the core-shell nano-modified microspheres specifically comprises the following steps: (1) Pour 2.0 g of silica particles into a 500 mL three-necked flask, add 50-100 mL of a mixed liquid of anhydrous ethanol and pure water, wherein the volume ratio of anhydrous ethanol to pure water is 3:1, then add 0.8 g of modifier KH-570, and adjust the pH to 4.0 with a hydrochloric acid solution with a mass fraction of 5.0-10.0%, ultrasonicate for 25-45 min, heat to 40-50 ° C, react for 1-2 h, centrifuge to obtain a precipitate, wash it with anhydrous ethanol 3-5 times, and vacuum dry to obtain modified silica; (2) Add 0.7 g of Span 80 and 0.2 g of Tween 60 to 30.0 g of liquid paraffin, stir evenly until completely dispersed, and use as the oil phase. Then add the modified silica described in step (1), 4.0 g of acrylic acid, 4.0 g of acrylamide, 0.55 g of 2-acrylamide-2-methylpropanesulfonic acid and 0.015 g of N,N-methylenebisacrylamide to 20.0 g of water, stir until completely dissolved, and adjust the mixture with 5.0% sodium bicarbonate solution. The pH value is adjusted to 7.0, which is used as the aqueous phase. At 40-50°C, 0.008g of ammonium persulfate and 0.008g of sodium bisulfite are dissolved in 1-2mL of distilled water, and then added dropwise to a three-necked flask. The oil phase and the aqueous phase are mixed, stirred evenly, and then poured into the flask. Nitrogen is passed through to deoxygenate, and the reaction is continued for 3-4h after stirring for 10-15min. The crude product is obtained by demulsification, suction filtration, and centrifugation, and then washed with anhydrous ethanol for 3-5 times and vacuum dried to obtain core-shell nano-modified microspheres.
5. The method for preparing the novel sol resin slurry according to claim 4, characterized in that: In step (2), the amount of modified silica added is 0.7-0.8 g.
6. The method for preparing the novel sol resin slurry according to claim 5, characterized in that: The preparation method of the composite super absorbent resin specifically comprises the following steps: a. Add 1.0 g of montmorillonite to 100 mL of water, stir at 100-300 rpm for 8-12 h, place in an ultrasonic cell disruptor, ultrasonicate at 350-450 W for 3-5 min, then add 0.1 g of octadecyl trimethyl ammonium bromide, stir at 40-50 ° C for 3-5 h, wash the reduced montmorillonite with anhydrous ethanol, add to 200 mL of water and stir to obtain a nano-montmorillonite suspension; b. Add 0.2 mL of 1.0-2.0% 3-aminopropyltriethoxysilane aqueous solution dropwise to the nano-montmorillonite suspension in step a at a constant temperature of 50° C. and stir for 24 hours. After the reaction is completed, centrifuge at a speed of 5000 rpm for 3-5 minutes, wash the precipitate with anhydrous ethanol for 3-5 times, and dry in vacuo to obtain amination montmorillonite; c. Add 8.0g starch and 2.0g amination montmorillonite described in step b to 50mL water, and gelatinize at 50-60℃ for 0.5-1h for standby use. Then weigh 5.0g acrylic acid in a conical flask containing 20mL distilled water, and dropwise add 10-20mL of 10% sodium hydroxide solution in an ice-water bath. After neutralization, add 1.0g 2-acrylamide-2-methylpropanesulfonic acid, stir evenly, and use as a monomer. Then add 0.7g Span 80 and 0.2g Tween 60 to 30. 0g liquid paraffin, mechanically stir at a constant temperature of 45-55℃ for 0.5-1h, after forming a stable oil phase, slowly add starch and amino montmorillonite solution into the oil phase, emulsify at 45-55℃ for 0.5-1h, finally add monomer, 2.0g potassium persulfate and 0.04g N,N-methylenebisacrylamide in sequence, first use an ultrasonic instrument to degas, then stir and react at 45-55℃ for 2-3h, cool the product to room temperature, wash with distilled water 3-5 times, vacuum filter, dry and grind to obtain a composite highly absorbent resin.
7. The method for preparing the novel sol resin slurry according to claim 6, characterized in that: In step a, the amount of octadecyltrimethylammonium bromide added is 1.0 g.
Citation Information
Patent Citations
Method for preparing acrylic acid series semi-interpenetration network composite high water absorption resin
CN101240052A
Water-swellable epoxy material
CN105237956A
Preparation method for vinyl polymer coated nano-silica microsphere and modified epoxy resin
CN106589464A
Composite material capable of realizing biodegradation, and preparation method and application thereof
CN106750553A
Concrete crack-filling epoxy resin glue
CN109135584A