Two-component epoxy resin for vacuum diversion and preparation method thereof

Through the design of two-component epoxy resin, the problem of dull surface and insufficient weather resistance of carbon fiber products in the vacuum diversion process is solved, and high-strength, high toughness and bright and transparent products are achieved, suitable for large-scale production.

CN118931115AActive Publication Date: 2024-11-12东莞市力源复合材料有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411184003.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

After the existing carbon fiber is processed with vacuum diversion epoxy resin, the product surface is dull, the number of micropores is large, and the weather resistance is insufficient, which is not conducive to subsequent surface painting processing and the toughness fails to meet the requirements.

Method used

Two-component epoxy resin is used, component A includes bisphenol A-type epoxy resin, bisphenol F-type epoxy resin and polyurethane modified epoxy resin, component B includes polyether amine curing agent, alicyclic amine The curing agent and benzyl alcohol are mixed in a specific proportion to form a resin with low viscosity and good fluidity. It is prepared by a vacuum flow diversion process. After curing, the product surface is bright and poreless, and has good weather resistance. It is suitable for large-scale production.

Benefits of technology

It achieves the bright surface of carbon fiber products, high transparency, good weather resistance, better strength and toughness, which is convenient for subsequent surface painting processing, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013014560000021
    Figure BDA0005013014560000021
  • Figure BDA0005013014560000051
    Figure BDA0005013014560000051
  • Figure BDA0005013014560000071
    Figure BDA0005013014560000071
Patent Text Reader

Abstract

The invention relates to the technical field of epoxy resin, in particular to two-component epoxy resin for vacuum diversion and a preparation method thereof.The two-component epoxy resin is composed of a component A and a component B. The weight ratio of the component A to the component B is 100: (20-30). After curing, a carbon fiber product is bright in surface, free of pores, good in weather resistance, bright in surface and high in transparency; and subsequent surface paint spraying processing is facilitated, the strength is better, and the toughness is better. Under the combined action of the polyurethane modified epoxy resin, the inorganic filler, the defoaming agent and the flatting agent, the dispersity of the component A is improved, a cured surface can be promoted to present a soft, flat and non-porous effect, the surface brightness and transparency of a product are facilitated, and the strength and toughness are improved. Under the action of benzyl alcohol, the component B contributes to improving the fluidity of epoxy resin, promoting reaction and improving toughness, and under the combined action of the component B and the component A, the gloss and brightness of the surface of a product can be remarkably improved, and subsequent surface paint spraying processing is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resins, and in particular to a two-component epoxy resin for vacuum conduction and a preparation method thereof. Background Art

[0002] Vacuum infusion (also known as VARTM, SCRIMP, VIP, etc.) is a lamination process for producing fiber reinforced plastic (FRP) parts. The process uses atmospheric pressure to press resin into dry materials (such as felt, fabric, stitched felt and foam core) under high vacuum. The pressure difference between the vacuum gap and the external atmospheric pressure presses the resin into the porous material until it is completely infiltrated. The vacuum is maintained until the part is cured, thereby manufacturing a dense composite part.

[0003] However, after the existing carbon fiber is processed with vacuum-infused epoxy resin, the product surface becomes dull, has a large number of micropores, and has insufficient weather resistance due to the influence of the composite materials in the epoxy resin, which is not conducive to subsequent processing operations such as surface painting, and the toughness fails to meet the requirements. Summary of the invention

[0004] In order to overcome the shortcomings and deficiencies in the prior art, one of the objectives of the present invention is to provide a two-component epoxy resin for vacuum infusion.

[0005] The second object of the present invention is to provide a method for preparing a two-component epoxy resin for vacuum infusion, which has simple operation, convenient control, high production efficiency, low production cost, and can be used for large-scale production.

[0006] One of the purposes of the present invention is achieved by the following technical solution: A two-component epoxy resin for vacuum infusion, comprising component A and component B in a weight ratio of 100:20-30;

[0007] The A component includes the following raw materials in parts by weight:

[0008] Bisphenol A epoxy resin 50-80 parts

[0009] Bisphenol F epoxy resin 15-25 parts

[0010] Polyurethane modified epoxy resin 8-12 parts

[0011]

[0012] The B component includes the following raw materials in parts by weight:

[0013] 10-20 parts of polyetheramine curing agent

[0014] Alicyclic amine curing agent 20-30 parts

[0015] Benzyl alcohol 10-12 parts.

[0016] The two-component epoxy resin used for vacuum infusion has component A as the main resin component and component B as the main curing component. After mixing in proportion, it has low viscosity and good fluidity, and is suitable for vacuum infusion. After curing, the surface of the carbon fiber product is bright and free of pores, with good weather resistance, bright surface and high transparency, which is more conducive to the subsequent surface painting processing, and has better strength and toughness. Among them, bisphenol A epoxy resin is used as the main resin in component A, bisphenol F epoxy resin and epoxy diluent are added to jointly reduce the overall viscosity of component A, and component A and component B jointly control the viscosity of the two-component epoxy resin at 500-800mPa·s, and the blend of bisphenol F epoxy resin, bisphenol A epoxy resin and polyurethane modified epoxy resin synergistically plays a good weather resistance and aging resistance. Under the joint action of special polyurethane modified epoxy resin, inorganic filler, defoamer and leveling agent, it is beneficial to improve the dispersibility of component A and promote the soft, flat and non-porous effect of the cured surface, which is beneficial to the brightness and transparency of the product surface and is more beneficial to improve the strength and toughness. In component B, polyetheramine curing agent and alicyclic amine curing agent are used to synergistically cure the two-component epoxy resin, which promotes the curing speed and is beneficial to improving weather resistance, water resistance, surface transparency and mechanical properties. Under the action of benzyl alcohol, it is helpful to improve the fluidity of the epoxy resin, promote the reaction of polyetheramine curing agent and alicyclic amine curing agent with the epoxy resin of component A, and improve the toughness of the cured product. In addition, under the joint action of the special polyurethane modified epoxy resin, inorganic filler, defoamer and leveling agent of component A, the gloss and transparency of the product surface can be significantly improved, which is more conducive to the subsequent surface spray painting process.

[0017] Preferably, the bisphenol A epoxy resin is E44; the bisphenol F epoxy resin is EXA-830CRP or EXA-830LVP.

[0018] Preferably, the preparation method of each portion of the polyurethane-modified epoxy resin comprises the following steps:

[0019] (R1), take 2.5-3.5 parts of polyether polyol, 8.5-9.5 parts of isocyanate, 85-95 parts of epoxy resin E44, 8-12 parts of terminal hydroxyl hyperbranched polyester and 1-2 parts of organotin catalyst by weight, and set aside;

[0020] (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 60-120° C. and stirring for 2-3 hours, and then cooling to room temperature to obtain a polyurethane prepolymer;

[0021] (R3), preheating epoxy resin E44 at 100-140° C. for 4-6 hours to remove moisture and volatiles therein, and evacuating the mixture until bubbles are eliminated to obtain a pretreated epoxy resin;

[0022] (R4), adding a polyurethane prepolymer, a terminal hydroxyl hyperbranched polyester and an organic tin catalyst to the pretreated epoxy resin, raising the temperature to 100-140°C, and performing high-speed homogeneous shear stirring at 1000-1500 rpm for 1 hour, continuing the reaction for 3-6 hours, and then evacuating and maintaining the vacuum for 15 minutes to remove bubbles in the liquid, thereby obtaining the polyurethane modified epoxy resin.

[0023] The polyurethane-modified epoxy resin is prepared by adopting the above technical scheme. The rigid molecules of the polyurethane-modified epoxy resin can be evenly dispersed in the epoxy matrix at the molecular level to form a molecular composite material. The whole system is similar to a semi-interpenetrating network. These rigid molecules can strengthen the matrix and improve the tensile strength of the matrix. At the same time, they can prevent cracks and increase the toughness of the matrix, and promote the cured surface to present a soft, flat and non-porous effect. The end-hydroxyl hyperbranched polyester is then introduced to further enhance the strength and toughness.

[0024] Preferably, the polyether polyol is polyethylene glycol or polyoxypropylene glycol; the isocyanate is at least one of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate.

[0025] Preferably, the terminal hydroxyl hyperbranched polyester is H303; and the organotin catalyst is dibutyltin dilaurate.

[0026] Preferably, the epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether.

[0027] Using the above technical solution, more preferably, the epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether in a weight ratio of 1-3:5, which is beneficial to improving heat resistance. The molecule of glycidyl methacrylate contains both carbon-carbon double bonds and epoxy groups, and the unique structure and steric hindrance of 2-toluene glycidyl ether can significantly improve the toughness and impact resistance of the cured epoxy resin, thereby enhancing the mechanical properties of the overall material.

[0028] Preferably, the inorganic filler is quartz powder and glass powder.

[0029] Using the above technical solution, more preferably, the inorganic filler is a mixture of ultrafine quartz powder and T836 glass powder in a weight ratio of 1-2:8. The two work synergistically, have high surface energy in the system, good compatibility, and good filling effect, effectively improve impact strength and tensile strength, and promote surface transparency and weather resistance.

[0030] Preferably, the defoaming agent is BYK-A530 or ACP-1400, and the leveling agent is polydimethylsiloxane or polymethylphenylsiloxane.

[0031] By adopting the above technical scheme, the above defoaming agent is resistant to high temperature, acid and alkali, has low toxicity, and has good dispersibility, and can effectively inhibit the formation of bubbles; the above leveling agent can significantly improve the leveling of the system, while improving the gloss and feel of the product surface.

[0032] Preferably, the polyetheramine curing agent is D-230; the alicyclic amine curing agent is 1,3-cyclohexanedimethylamine and isophoronediamine.

[0033] Using the above technical solution, more preferably, the alicyclic amine curing agent is a mixture of 1,3-cyclohexanedimethylamine and isophoronediamine in a weight ratio of 3:1-2, which has faster curing speed, better low-temperature weather resistance, better water resistance, and yellowing resistance. It has the characteristics of low viscosity, clearness, good mechanical properties and excellent weather resistance, and can significantly improve production efficiency and improve product quality.

[0034] The second object of the present invention is achieved by the following technical solution: The preparation method of the above-mentioned two-component epoxy resin for vacuum infusion comprises the following steps:

[0035] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A;

[0036] (S2), taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol in parts by weight, mixing them evenly, filtering and removing impurities, and obtaining a component B;

[0037] When the two-component epoxy resin is used in a vacuum infusion process, component A and component B are uniformly mixed according to a weight ratio, and the obtained two-component epoxy resin is introduced into a mold with a carbon fiber product by vacuuming, and then cured at room temperature for 23-25 ​​hours or heated to 60-70°C for 30-60 minutes.

[0038] The beneficial effects of the present invention are as follows: the two-component epoxy resin for vacuum infusion of the present invention has component A as the main resin component and component B as the main curing component. After being mixed in proportion, the viscosity is low and the fluidity is good, and the product is suitable for vacuum infusion. After curing, the surface of the carbon fiber product is bright and free of pores, and the product has good weather resistance, bright surface and high transparency, which is more conducive to the subsequent surface spray painting processing, and has better strength and toughness.

[0039] The preparation method of the invention has the advantages of simple operation, convenient control, high production efficiency and low production cost, and can be used for large-scale production. DETAILED DESCRIPTION

[0040] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0041] Example 1

[0042] A two-component epoxy resin for vacuum infusion, comprising component A and component B in a weight ratio of 100:25;

[0043] The A component includes the following raw materials in parts by weight:

[0044]

[0045] The B component includes the following raw materials in parts by weight:

[0046] 15 parts of polyetheramine curing agent

[0047] Alicyclic amine curing agent 25 parts

[0048] Benzyl alcohol 11 parts.

[0049] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is EXA-830CRP.

[0050] The preparation method of each polyurethane modified epoxy resin comprises the following steps:

[0051] (R1), take 3 parts of polyether polyol, 9 parts of isocyanate, 90 parts of epoxy resin E44, 10 parts of terminal hydroxyl hyperbranched polyester and 1.5 parts of organotin catalyst by weight, and set aside;

[0052] (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 90° C. and stirring for 2.5 h, and then cooling to room temperature to obtain a polyurethane prepolymer;

[0053] (R3), preheating the epoxy resin E44 at 120° C. for 5 h to remove moisture and volatiles therein, and evacuating the mixture until bubbles are eliminated to obtain a pretreated epoxy resin;

[0054] (R4), add polyurethane prepolymer, terminal hydroxyl hyperbranched polyester and organic tin catalyst to the pretreated epoxy resin, raise the temperature to 120°C, and stir at 1200 rpm for 1 hour, continue the reaction for 4 hours, then evacuate and maintain for 15 minutes to remove bubbles in the liquid, thereby obtaining the polyurethane modified epoxy resin.

[0055] The polyether polyol is polyoxypropylene glycol; the isocyanate is a mixture of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate in a weight ratio of 1:2:1.

[0056] The terminal hydroxyl hyperbranched polyester is H303; the organic tin catalyst is dibutyltin dilaurate.

[0057] The epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether in a weight ratio of 2:5.

[0058] The inorganic filler is a mixture of ultrafine quartz powder and T836 glass powder in a weight ratio of 1.5:8.

[0059] The defoamer is BYK-A530, and the leveling agent is polydimethylsiloxane.

[0060] The polyetheramine curing agent is D-230; the alicyclic amine curing agent is a mixture of 1,3-cyclohexanedimethylamine and isophoronediamine in a weight ratio of 3:1.5.

[0061] The method for preparing the two-component epoxy resin for vacuum infusion comprises the following steps:

[0062] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A;

[0063] (S2) taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol by weight, mixing them evenly, filtering and removing impurities, and obtaining component B.

[0064] Example 2

[0065] A two-component epoxy resin for vacuum infusion, comprising component A and component B in a weight ratio of 100:20;

[0066] The A component includes the following raw materials in parts by weight:

[0067]

[0068] The B component includes the following raw materials in parts by weight:

[0069] 10 parts of polyetheramine curing agent

[0070] Alicyclic amine curing agent 20 parts

[0071] Benzyl alcohol 10 parts.

[0072] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is EXA-830CRP.

[0073] The preparation method of each polyurethane modified epoxy resin comprises the following steps:

[0074] (R1), take 2.5 parts of polyether polyol, 8.5 parts of isocyanate, 85 parts of epoxy resin E44, 8 parts of terminal hydroxyl hyperbranched polyester and 1 part of organotin catalyst by weight, and set aside;

[0075] (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 60° C. and stirring for 2 h, and then cooling to room temperature to obtain a polyurethane prepolymer;

[0076] (R3), preheating the epoxy resin E44 at 100° C. for 4 h to remove moisture and volatiles therein, and evacuating the mixture until bubbles are eliminated to obtain a pretreated epoxy resin;

[0077] (R4), adding a polyurethane prepolymer, a terminal hydroxyl hyperbranched polyester and an organic tin catalyst to the pretreated epoxy resin, heating to 100°C, and high-speed homogeneous shear stirring at 1000 rpm for 1 hour, continuing the reaction for 3 hours, and then evacuating and maintaining for 15 minutes to remove bubbles in the liquid, thereby obtaining the polyurethane modified epoxy resin.

[0078] The polyether polyol is polyoxypropylene glycol; the isocyanate is a mixture of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate in a weight ratio of 1:2:1.

[0079] The terminal hydroxyl hyperbranched polyester is H303; the organic tin catalyst is dibutyltin dilaurate.

[0080] The epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether in a weight ratio of 1:5.

[0081] The inorganic filler is a mixture of ultrafine quartz powder and T836 glass powder in a weight ratio of 1:8.

[0082] The defoaming agent is ACP-1400, and the leveling agent is polymethylphenylsiloxane.

[0083] The polyetheramine curing agent is D-230; the alicyclic amine curing agent is a mixture of 1,3-cyclohexanedimethylamine and isophoronediamine in a weight ratio of 3:1.

[0084] The method for preparing the two-component epoxy resin for vacuum infusion comprises the following steps:

[0085] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A;

[0086] (S2) taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol by weight, mixing them evenly, filtering and removing impurities, and obtaining component B.

[0087] Example 3

[0088] A two-component epoxy resin for vacuum infusion, comprising component A and component B in a weight ratio of 100:30;

[0089] The A component includes the following raw materials in parts by weight:

[0090]

[0091] The B component includes the following raw materials in parts by weight:

[0092] 20 parts of polyetheramine curing agent

[0093] 30 parts of alicyclic amine curing agent

[0094] Benzyl alcohol 12 parts.

[0095] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is EXA-830CRP.

[0096] The preparation method of each polyurethane modified epoxy resin comprises the following steps:

[0097] (R1), take 3.5 parts of polyether polyol, 9.5 parts of isocyanate, 95 parts of epoxy resin E44, 12 parts of terminal hydroxyl hyperbranched polyester and 2 parts of organotin catalyst by weight, and set aside;

[0098] (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 120° C. and stirring for 3 h, and then cooling to room temperature to obtain a polyurethane prepolymer;

[0099] (R3), preheating the epoxy resin E44 at 140° C. for 6 h to remove moisture and volatiles therein, and evacuating the mixture until bubbles are eliminated to obtain a pretreated epoxy resin;

[0100] (R4), add polyurethane prepolymer, terminal hydroxyl hyperbranched polyester and organic tin catalyst to the pretreated epoxy resin, raise the temperature to 140°C, and stir the mixture at 1500 rpm for 1 hour, continue the reaction for 6 hours, then evacuate and maintain for 15 minutes to remove bubbles in the liquid, thereby obtaining the polyurethane modified epoxy resin.

[0101] The polyether polyol is polyoxypropylene glycol; the isocyanate is a mixture of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate in a weight ratio of 1:2:1.

[0102] The terminal hydroxyl hyperbranched polyester is H303; the organic tin catalyst is dibutyltin dilaurate.

[0103] The epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether in a weight ratio of 3:5.

[0104] The inorganic filler is a mixture of ultrafine quartz powder and T836 glass powder in a weight ratio of 2:8.

[0105] The defoamer is BYK-A530, and the leveling agent is polydimethylsiloxane.

[0106] The polyetheramine curing agent is D-230; the alicyclic amine curing agent is a mixture of 1,3-cyclohexanedimethylamine and isophoronediamine in a weight ratio of 3:2.

[0107] The method for preparing the two-component epoxy resin for vacuum infusion comprises the following steps:

[0108] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A;

[0109] (S2) taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol by weight, mixing them evenly, filtering and removing impurities, and obtaining component B.

[0110] Example 4

[0111] A two-component epoxy resin for vacuum infusion, comprising component A and component B in a weight ratio of 100:27;

[0112] The A component includes the following raw materials in parts by weight:

[0113] 70 parts of bisphenol A epoxy resin

[0114] 18 parts of bisphenol F epoxy resin

[0115] Polyurethane modified epoxy resin 11 parts

[0116] Epoxy diluent 16 parts

[0117] 14 parts of inorganic filler

[0118] Defoamer 0.7 parts

[0119] 0.4 parts of leveling agent;

[0120] The B component includes the following raw materials in parts by weight:

[0121] 17 parts of polyetheramine curing agent

[0122] Alicyclic amine curing agent 27 parts

[0123] Benzyl alcohol 11 parts.

[0124] The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is EXA-830CRP.

[0125] The preparation method of each polyurethane modified epoxy resin comprises the following steps:

[0126] (R1), take 2.8 parts of polyether polyol, 8.8 parts of isocyanate, 88 parts of epoxy resin E44, 11 parts of terminal hydroxyl hyperbranched polyester and 1.8 parts of organotin catalyst by weight, and set aside;

[0127] (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 88° C. and stirring for 2.3 h, and then cooling to room temperature to obtain a polyurethane prepolymer;

[0128] (R3), preheating the epoxy resin E44 at 130° C. for 4.5 h to remove moisture and volatiles therein, and evacuating the mixture until bubbles are eliminated to obtain a pretreated epoxy resin;

[0129] (R4), add polyurethane prepolymer, terminal hydroxyl hyperbranched polyester and organic tin catalyst to the pretreated epoxy resin, heat to 130°C, and stir at 1300 rpm for 1 hour, continue to react for 4.5 hours, then evacuate and maintain for 15 minutes to remove bubbles in the liquid, to obtain the polyurethane modified epoxy resin.

[0130] The polyether polyol is polyoxypropylene glycol; the isocyanate is a mixture of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate in a weight ratio of 1:2:1.

[0131] The terminal hydroxyl hyperbranched polyester is H303; the organic tin catalyst is dibutyltin dilaurate.

[0132] The epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether in a weight ratio of 2.3:5.

[0133] The inorganic filler is a mixture of ultrafine quartz powder and T836 glass powder in a weight ratio of 1.3:8.

[0134] The defoamer is BYK-A530, and the leveling agent is polydimethylsiloxane.

[0135] The polyetheramine curing agent is D-230; the alicyclic amine curing agent is a mixture of 1,3-cyclohexanedimethylamine and isophoronediamine in a weight ratio of 3:1.3.

[0136] The method for preparing the two-component epoxy resin for vacuum infusion comprises the following steps:

[0137] (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A;

[0138] (S2) taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol by weight, mixing them evenly, filtering and removing impurities, and obtaining component B.

[0139] Comparative Example 1

[0140] The difference between this comparative example and Example 1 is:

[0141] In the preparation method of each part of the polyurethane-modified epoxy resin, in step (R1), 3 parts of polyether polyol, 9 parts of isocyanate, 100 parts of epoxy resin E44, 0 parts of terminal hydroxyl hyperbranched polyester and 1.5 parts of organic tin catalyst are taken by weight and set aside; that is, the polyurethane-modified epoxy resin does not contain terminal hydroxyl hyperbranched polyester.

[0142] Comparative Example 2

[0143] The difference between this comparative example and Example 1 is:

[0144] The epoxy diluent is a mixture of neopentyl glycol diglycidyl ether and 1,4-butanediol diglycidyl ether in a weight ratio of 2:5.

[0145] Comparative Example 3

[0146] The difference between this comparative example and Example 1 is:

[0147] The inorganic filler is nano silicon dioxide.

[0148] Comparative Example 4

[0149] The difference between this comparative example and Example 1 is:

[0150] The B component includes the following raw materials in parts by weight:

[0151] 21 parts of polyetheramine curing agent

[0152] 30 parts of alicyclic amine curing agent

[0153] 0 parts of benzyl alcohol; that is, component B does not contain benzyl alcohol.

[0154] Example 5 Performance Test

[0155] Take the two-component epoxy resins of Examples 1-4 and Comparative Examples 1-4, and when preparing the sample, mix the A component and the B component of the two-component epoxy resin evenly according to the weight ratio, and introduce the obtained two-component epoxy resin into a mold with a ZT6F carbon fiber product by vacuuming, and then heat it to 65°C and cure it for 45 minutes to obtain the sample. Test its tensile strength, bending strength, surface flatness and surface gloss after vacuum induction and carbon fiber product curing; the test method is as follows:

[0156] Tensile strength: The tensile strength of the sample was tested according to ASTM D3039 Standard Test Method for Tensile Properties of Polymer Matrix Composites.

[0157] Bending strength: "ASTM D790 Standard Test Method for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials" is used to test the bending strength of the specimens.

[0158] Surface flatness: Take the sample and observe whether the surface is flat, smooth and has no obvious defects.

[0159] Surface gloss: Instrument model: HG60S gloss meter, incident angle: 60°, read the gloss value of the sample.

[0160] The test results are shown in Table 1 below:

[0161]

[0162]

[0163] As can be seen from Table 1 above, the two-component epoxy resin for vacuum infusion of the present invention has component A as the main resin component and component B as the main curing component. After being mixed in proportion, it has low viscosity and good fluidity, is suitable for vacuum infusion, and after curing, the surface of the carbon fiber product is bright and free of pores, has good weather resistance, bright surface and high transparency, is more conducive to the subsequent surface painting process, and has better strength and toughness.

[0164] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A two-component epoxy resin for vacuum infusion, characterized in that: It is composed of component A and component B in a weight ratio of 100:20-30; The A component includes the following raw materials in parts by weight: The B component includes the following raw materials in parts by weight: 10-20 parts of polyetheramine curing agent Alicyclic amine curing agent 20-30 parts Benzyl alcohol 10-12 parts.

2. A two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The bisphenol A type epoxy resin is E44; the bisphenol F type epoxy resin is EXA-830CRP or EXA-830LVP.

3. The two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The preparation method of each polyurethane modified epoxy resin comprises the following steps: (R1), take 2.5-3.5 parts of polyether polyol, 8.5-9.5 parts of isocyanate, 85-95 parts of epoxy resin E44, 8-12 parts of terminal hydroxyl hyperbranched polyester and 1-2 parts of organotin catalyst by weight, and set aside; (R2), adding polyether polyol and isocyanate into a reaction kettle, mixing, introducing nitrogen, heating to 60-120° C. and stirring for 2-3 hours, and then cooling to room temperature to obtain a polyurethane prepolymer; (R3), preheating epoxy resin E44 at 100-140° C. for 4-6 hours to remove moisture and volatiles therein, and evacuating until bubbles are eliminated to obtain a pretreated epoxy resin; (R4), adding a polyurethane prepolymer, a terminal hydroxyl hyperbranched polyester and an organic tin catalyst to the pretreated epoxy resin, raising the temperature to 100-140°C, and performing high-speed homogeneous shear stirring at 1000-1500 rpm for 1 hour, continuing the reaction for 3-6 hours, and then evacuating and maintaining the vacuum for 15 minutes to remove bubbles in the liquid, thereby obtaining the polyurethane modified epoxy resin.

4. A two-component epoxy resin for vacuum infusion according to claim 3, characterized in that: The polyether polyol is polyethylene glycol or polyoxypropylene glycol; the isocyanate is at least one of diphenylmethane diisocyanate, isophorone diisocyanate and p-phenylene diisocyanate.

5. The two-component epoxy resin for vacuum infusion according to claim 3, characterized in that: The terminal hydroxyl hyperbranched polyester is H303; and the organic tin catalyst is dibutyltin dilaurate.

6. The two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The epoxy diluent is a mixture of glycidyl methacrylate and 2-toluene glycidyl ether.

7. The two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The inorganic filler is quartz powder and glass powder.

8. The two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The defoaming agent is BYK-A530 or ACP-1400, and the leveling agent is polydimethylsiloxane or polymethylphenylsiloxane.

9. The two-component epoxy resin for vacuum infusion according to claim 1, characterized in that: The polyetheramine curing agent is D-230; the alicyclic amine curing agents are 1,3-cyclohexanedimethylamine and isophoronediamine.

10. A method for preparing a two-component epoxy resin for vacuum infusion according to any one of claims 1 to 9, characterized in that: The steps include: (S1), taking bisphenol A epoxy resin, bisphenol F epoxy resin, polyurethane modified epoxy resin, epoxy diluent, inorganic filler, defoamer and leveling agent by weight, mixing them evenly, evacuating until bubbles are eliminated, filtering and removing impurities, and obtaining component A; (S2), taking a polyetheramine curing agent, an alicyclic amine curing agent and benzyl alcohol in parts by weight, mixing them evenly, filtering and removing impurities, and obtaining a component B; When the two-component epoxy resin is used in a vacuum infusion process, component A and component B are uniformly mixed according to a weight ratio, and the obtained two-component epoxy resin is introduced into a mold with a carbon fiber product by vacuuming, and then cured at room temperature for 23-25 ​​hours or heated to 60-70°C for 30-60 minutes.

Citation Information

Patent Citations

  • Vacuum infusion resin for wind turbine blades and preparation method thereof

    CN101735564A

  • Curing agent for low temperature cure applications

    CN101781397A

  • Low-viscosity epoxy resin system for rapid repair and reinforcement and preparation method of low-viscosity epoxy resin system

    CN102746621A

  • Hardeners for low-emission epoxy resin products

    CN104884496A

  • Additives to resin compositions for improved impact strength and flexibility

    CN105705585A