Antifouling composite material as well as preparation method and application thereof
By using biodegradable polyurethane material and Elostone nanotube composite material loaded with antifouling agent, the heavy metal pollution and short-effect problems of marine antifouling materials are solved, and a long-term and environmentally friendly marine antifouling effect is achieved, suitable for the ocean Anti-fouling application of engineering equipment.
Patent Information
- Application Number
- CN202310523724.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing marine anti-fouling materials have problems such as heavy metal pollution, short-effect and microplastic pollution. Traditional methods cannot effectively prevent marine organisms from adhering and growing on the surface of marine engineering equipment.
The antifouling composite material is prepared by using degradable polyurethane material and antifouling agent-loaded Elosite nanotube composite material, and vacuum loading and ultrasonic dispersion technology to form a long-term antifouling layer to prevent marine organisms from adhesion and growth.
It achieves a green, environmentally friendly and long-term marine anti-fouling effect, avoids heavy metal pollution, extends the release time of anti-fouling agent, improves the anti-fouling ability of dynamic and static surfaces, and is suitable for anti-fouling in static waters.
Smart Images

Figure CN118931164A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of functional composite materials, and more particularly to an antifouling composite material and a preparation method and application thereof. Background Art
[0002] Marine biofouling refers to the biofouling formed by the adsorption, growth and reproduction of marine microorganisms, plants and animals on the surface of objects immersed in seawater. It can cause great harm to marine engineering equipment such as ships, nuclear power plants, and oil platforms. If no protective measures are taken, a large amount of dirt will accumulate and adhere to the bottom of the ship in a short period of time, which will reduce the speed of the ship, increase fuel consumption, reduce the service life of the hull, and cause great economic losses in subsequent maintenance.
[0003] Marine antifouling is the use of physical or chemical methods to prevent marine organisms from attaching and growing on the surface of objects, or to make them detach from the surface. Traditional antifouling coatings kill marine organisms by releasing toxic materials such as tin, mercury, and lead. Studies have found that heavy metals can accumulate in a variety of fish, shellfish, and marine plants for a long time, leading to genetic mutations and entering the food chain, causing immeasurable ecological problems. Therefore, the development of green and efficient antifouling materials that do not contain heavy metals is of great practical significance.
[0004] The degradation of existing self-polishing antifouling materials depends on the shear and tearing effect of external forces, and it is necessary to rely on seawater scouring to achieve surface self-polishing, thereby removing contaminants and achieving an antifouling effect, which is very unfriendly to facilities fixed in seawater; in addition, it is mainly the side groups that undergo hydrolysis to produce small molecules, and the main chain will exist in the ocean for a long time due to its non-degradability, causing microplastic pollution. In order to achieve a better antifouling effect, antifouling agents are generally compounded, but antifouling agents are generally directly combined with the matrix by physical blending, and will migrate to the coating surface in a short time and be completely released, which greatly reduces the antifouling effect. Therefore, it is necessary to develop an environmentally friendly and long-lasting marine antifouling material. Summary of the invention
[0005] In order to solve the above problems, the present invention provides an antifouling composite material and its preparation method and application. The present invention adopts a degradable polyurethane material and a slow-release filler to prepare an antifouling composite material. The polyurethane can be continuously degraded into non-toxic small molecules, and the slow-release filler can release antifouling agents for a long time. The combination of the two ensures that the surface of the composite material is continuously dynamically updated, and ensures the excellent dynamic / static long-term antifouling performance of the composite material. The antifouling composite material provided by the present invention can be coated on the surface of marine engineering equipment to form a long-term protective circle around the marine engineering equipment to prevent marine organisms from attaching or growing on the surface of the equipment.
[0006] Firstly, one of the objectives of the present invention is to provide an antifouling composite material.
[0007] The antifouling composite material is prepared from raw materials including the following components, and each component is calculated by weight:
[0008] The polymer matrix is 100 parts by weight. The polymer matrix is a polyurethane polymer whose main chain can be degraded into non-toxic small molecules, and is preferably one of polycaprolactone polyurethane, polylactic acid polyurethane and polycarbonate polyurethane.
[0009] The slow-release filler is 1 to 100 parts by weight, preferably 1 to 60 parts by weight. The slow-release filler is halloysite nanotubes loaded with an antifouling agent. Preferably, the antifouling agent is one selected from maleimide, isothiazolinone, and capsaicin antifouling agents.
[0010] Further, the polymer matrix is prepared by the following method:
[0011] The polyester polyol, diisocyanate and catalyst are mixed and reacted to obtain a prepolymer, and then a chain extender is added to react to obtain a degradable polymer matrix.
[0012] The following steps can be used:
[0013] The polyester polyol is dehydrated in vacuo at 115°C, and then cooled to 80°C. Diisocyanate and a catalyst are added under normal pressure and a nitrogen atmosphere. A prepolymer is obtained after a period of reaction. A chain extender is added to continue the reaction. After the reaction is completed, the product is placed in a vacuum oven for curing. The curing temperature is controlled at 80-110°C to obtain a degradable polyurethane matrix.
[0014] Preferably, the polyester polyol is one of polycaprolactone diol, polypropylene carbonate diol, and poly-L-lactide diol; the diisocyanate is one of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate; the catalyst is one of dimethylcyclohexylamine and dibutyltin dilaurate; and the chain extender is one of 1,4-butanediol, 1,6-hexanediol, and ethylene glycol.
[0015] Further, the antifouling agent-loaded halloysite nanotubes are prepared by the following method:
[0016] Step 1: placing the halloysite nanotubes in a muffle furnace and treating them at a high temperature of 120 to 1000° C. for 1 to 3 hours;
[0017] Step 2, dissolving the antifouling agent in a solvent to prepare an antifouling agent solution with a concentration of 10 to 150 g / L, wherein the solvent is selected from one of ethanol and xylene;
[0018] Step 3, adding the halloysite nanotubes treated in step 1 to the antifouling agent solution prepared in step 2 to prepare a suspension, and subjecting the suspension to ultrasonic dispersion treatment to make the concentration of halloysite in the suspension 5 to 300 g / L;
[0019] Step 4: Using a vacuum loading method, the suspension prepared in step 3 is stirred 3 to 5 times under vacuum / normal pressure, and then centrifuged, washed, dried, and ground to obtain the antifouling agent-loaded halloysite nanotubes, wherein the vacuum pressure is -0.095 to -0.01 MPa, the centrifugal speed is 5000 to 8000 r / min, and the drying temperature is 60 to 80°C.
[0020] Halloysite exists in nature in the form of nano hollow tubes, and its lumen can be loaded with functional preparations. However, when preparing composite materials with fillers of hollow tubular structures, the number of functional preparations loaded is lower than the number of functional preparations loaded with fillers of granular structures. At present, the main methods for preparing halloysite loaded with functional preparations are vacuum adsorption method (no stirring during the preparation process) or simple stirring adsorption method. Such methods have uneven loading and poor loading effects. In order to achieve a good functional preparation loading effect of halloysite, the present invention first uses ultrasound to disperse the halloysite nanotubes before loading, and adopts a method of mechanical stirring while circulating under vacuum / normal pressure during the loading process to achieve better dispersion. It can be seen from the test results of the thermogravimetric analysis curve that the halloysite nanotubes loaded with antifouling agents of the present invention have a good loading effect, and the theoretical loading rate can be reached by adjusting the raw material ratio.
[0021] Secondly, the second object of the present invention is to provide a method for preparing the antifouling composite material of the first object of the present invention.
[0022] The following steps are involved:
[0023] The antifouling composite material is prepared by blending the polymer matrix and the slow-release filler according to the required amount.
[0024] The following steps can be used:
[0025] The polymer matrix and the slow-release filler were mixed at 150° C. using a Haake internal mixer, and then hot-pressed to obtain an antifouling composite material.
[0026] Again, the third object of the present invention is to provide the application of the antifouling composite material of one of the objects of the present invention in marine engineering equipment.
[0027] The antifouling composite material provided by the present invention can be coated on the surface of marine engineering equipment to form a long-term protection circle around the marine engineering equipment to prevent marine organisms from attaching or growing on the surface of the equipment.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The antifouling composite material provided by the present invention is a green, environmentally friendly, slow-release composite material, which does not contain heavy metals, and the matrix can be degraded into non-toxic small molecules, which has no pollution to the marine environment. The degradation of the matrix does not rely on the scouring of strong water flow, and can achieve antifouling in static waters.
[0030] 2. The antifouling composite material provided by the present invention solves the problem of early burst release of the antifouling agent, prolongs the action time of the antifouling agent, reduces the amount of antifouling agent used, and prolongs the antifouling time.
[0031] 3. The antifouling composite material provided by the present invention has a polymer matrix main chain that can be degraded into non-toxic small molecules, which can achieve dynamic / static surface self-renewal, and the slow-release filler can prolong the release time of the antifouling agent, thereby constructing an eco-friendly antifouling system with excellent dynamic / static long-term antifouling ability; further, the present invention combines the two antifouling strategies of dynamic surface removal and slow-release antifouling agent by combining the slow-release filler with the degradable matrix, so that the antifouling composite material can achieve better antifouling effect.
[0032] 4. The antifouling composite material provided by the present invention adopts high-temperature treated halloysite nanotubes as a matrix, loads the antifouling agent into the halloysite tube cavity by vacuum loading and stirring, and finally composites the halloysite nanotubes loaded with the antifouling agent with a degradable polymer matrix, so that the antifouling composite material has good mechanical properties.
[0033] 5. The method for preparing the antifouling composite material provided by the present invention has readily available raw materials, a simple and easy process, and has broad application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The static hydrolysis curves of the degradable polycaprolactone polyurethane matrix prepared in Examples 1 to 4 of the present invention;
[0035] Figure 2 Thermogravimetric analysis curves of antifouling agent (TCPM) and halloysite (HNTs);
[0036] Figure 3 Thermogravimetric analysis curves of the antifouling agent-loaded halloysite nanotubes prepared in Examples 7 to 9 of the present invention;
[0037] Figure 4 It is a graph showing the antifouling agent release curve of the antifouling agent-loaded halloysite nanotubes (HNTs-TCPM) prepared in Example 8 of the present invention in different solvents;
[0038] Figure 5 The SEM (a) image and TEM (b) image of the antifouling composite material prepared in Example 12 of the present invention;
[0039] Figure 6The antifouling agent release curves of the antifouling composite material (PCLU / HNTs-TCPM) prepared in Example 12 of the present invention and the composite material (PCLU / TCPM) prepared in Comparative Example 1;
[0040] Figure 7 The SEM images of the sample surfaces of the composite materials prepared in Example 12, Example 13, Comparative Example 1 and Comparative Example 2 after being suspended in a culture solution of Vibrio natrii for three days, wherein (a) corresponds to the SEM image of Example 13, (b) corresponds to the SEM image of Comparative Example 2, (c) corresponds to the SEM image of Comparative Example 1, and (d) corresponds to the SEM image of Example 12;
[0041] Figure 8 These are SEM images of the sample surfaces of the composite materials prepared in Example 12 and Comparative Example 1 after being placed in artificial seawater for 60 days, wherein (a) corresponds to the SEM image of Comparative Example 1, and (b) corresponds to the SEM image of Example 12. DETAILED DESCRIPTION
[0042] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0043] Sources and models of raw materials used in the examples:
[0044]
[0045]
[0046] Example 1
[0047] This example is used to illustrate the preparation of a polycaprolactone polyurethane polymer matrix.
[0048] 30g of polycaprolactone diol was dehydrated in vacuo at 115°C, and then cooled to 80°C. 19.7g of hexamethylene diisocyanate and 0.0149g of dibutyltin dilaurate were added under normal pressure and nitrogen atmosphere. After a period of reaction, a prepolymer was obtained. 5.41g of 1,4-butanediol was added to continue the reaction. After the reaction was completed, the product was placed in a vacuum oven at 90°C for curing to obtain a degradable polycaprolactone polyurethane polymer matrix, abbreviated as PCLU-54.
[0049] Example 2
[0050] This example is used to illustrate the preparation of a polycaprolactone polyurethane polymer matrix.
[0051] 30g of polycaprolactone diol was dehydrated in vacuo at 115°C, and then cooled to 80°C. 11.2g of hexamethylene diisocyanate and 0.0124g of dibutyltin dilaurate were added under normal pressure and nitrogen atmosphere. After a period of reaction, a prepolymer was obtained. 2.51g of 1,4-butanediol was added to continue the reaction. After the reaction was completed, the product was placed in a vacuum oven at 90°C for curing to obtain a degradable polycaprolactone polyurethane polymer matrix, abbreviated as PCLU-68.
[0052] Example 3
[0053] This example is used to illustrate the preparation of a polycaprolactone polyurethane polymer matrix.
[0054] 30g of polycaprolactone diol was dehydrated in vacuo at 115°C, and then cooled to 80°C. 7.87g of hexamethylene diisocyanate and 0.0114g of dibutyltin dilaurate were added under normal pressure and nitrogen atmosphere. After a period of reaction, a prepolymer was obtained. 1.35g of 1,4-butanediol was added to continue the reaction. After the reaction was completed, the product was placed in a vacuum oven at 90°C for curing to obtain a degradable polycaprolactone polyurethane polymer matrix, abbreviated as PCLU-74.
[0055] Example 4
[0056] This example is used to illustrate the preparation of a polycaprolactone polyurethane polymer matrix.
[0057] 30g of polycaprolactone diol was dehydrated in vacuo at 115°C, and then cooled to 80°C. 4.92g of hexamethylene diisocyanate and 0.0105g of dibutyltin dilaurate were added under normal pressure and nitrogen atmosphere. After a period of reaction, a prepolymer was obtained. 0.338g of 1,4-butanediol was added to continue the reaction. After the reaction was completed, the product was placed in a vacuum oven at 90°C for curing to obtain a degradable polycaprolactone polyurethane polymer matrix, abbreviated as PCLU-85.
[0058] Figure 1 This is the static hydrolysis curve of the degradable polycaprolactone polyurethane matrix prepared in Examples 1 to 4 above.
[0059] As can be seen from the figure, the polycaprolactone polyurethane (PCLU) prepared in Examples 1 to 4 can all achieve degradation performance, and when used as the matrix of the composite material, it can achieve dynamic surface self-renewal to remove surface contaminants. Further, it can be seen from the figure that the degradation rate is different for different soft segment contents in the polymer matrix. Among them, the hydrolysis rate of the polycaprolactone polyurethane (PCLU-74) prepared in Example 3 is the fastest, the hydrolysis rate of the polycaprolactone polyurethane (PCLU-68) prepared in Example 2 is slightly worse, and the hydrolysis rate of the polycaprolactone polyurethane prepared in Examples 1 and 4 is the slowest. This is because on the one hand, the increase in the content of polycaprolactone (PCL) will increase the crystallinity of the polymer (PCLU), weakening its hydrolysis ability; on the other hand, the increase in the content of polycaprolactone (PCL) increases the hydrolyzable ester group, enhancing its hydrolysis ability. The two-sided influence leads to the fastest hydrolysis rate of the polymer (PCLU-74) prepared in Example 3. It is inferred from the figure that it takes at least three years for the polymer (PCLU-74) prepared in Example 3 to be completely degraded.
[0060] Example 5
[0061] This example is used to illustrate the preparation of a polylactic acid ester polyurethane polymer matrix (PLLAU).
[0062] The preparation methods of this embodiment are basically the same as those of embodiment 3, except that the soft segment selected in this embodiment is poly-L-lactide diol, the isocyanate is hexamethylene diisocyanate, the chain extender is ethylene glycol, and the catalyst is dimethylcyclohexylamine.
[0063] Example 6
[0064] This example is used to illustrate the preparation of polypropylene carbonate polyurethane polymer matrix (PPCU).
[0065] The preparation methods of this embodiment are basically the same as those of embodiment 3, except that the soft segment selected in this embodiment is polypropylene carbonate diol, the isocyanate selected isophorone diisocyanate, and the chain extender selected is 1,6-hexanediol.
[0066] Example 7
[0067] This example is used to illustrate the preparation of halloysite nanotubes loaded with N-(2,4,6-trichlorophenyl)maleimide antifouling agent.
[0068] The halloysite nanotubes were placed in a muffle furnace and treated at 550°C for 3 hours. The antifouling agent N-(2,4,6-trichlorophenyl)maleimide (TCPM) was dissolved in ethanol to prepare an antifouling agent solution with a concentration of 25 g / L. The treated halloysite nanotubes were added to the antifouling agent solution to prepare a suspension. The suspension was dispersed in ultrasound. The concentration of halloysite in the suspension was 50 g / L. The vacuum loading method was used with a vacuum loading pressure of -0.01 MPa. The suspension was stirred three times under vacuum / normal pressure. After completion, the suspension was centrifuged at 8000 r / min, washed, dried at 70°C, and ground to obtain halloysite nanotubes loaded with N-(2,4,6-trichlorophenyl)maleimide antifouling agent, abbreviated as HNTs-TCPM.
[0069] Example 8
[0070] This example is used to illustrate the preparation of halloysite nanotubes loaded with N-(2,4,6-trichlorophenyl)maleimide antifouling agent.
[0071] The preparation methods of this embodiment are substantially the same as those of embodiment 7, except that the concentration of halloysite in the suspension of this embodiment is 25 g / L.
[0072] Furthermore, the antifouling agent release process of the antifouling agent-loaded halloysite nanotubes (HNTs / TCPM) prepared in Example 8 was tested.
[0073] The specific steps are as follows:
[0074] 100 mg of the antifouling agent-loaded halloysite nanotubes prepared in Example 8 were placed in 2 ml of deionized water or cyclohexane and stirred. The solution was separated by centrifugation at regular intervals and then new solvent was added. The supernatant was analyzed by UV-visible absorption spectroscopy to obtain an antifouling agent release curve, as shown in FIG. Figure 4 shown.
[0075] Example 9
[0076] This example is used to illustrate the preparation of halloysite nanotubes loaded with N-(2,4,6-trichlorophenyl)maleimide antifouling agent.
[0077] The preparation methods of this embodiment are substantially the same as those of embodiment 7, except that the concentration of halloysite in the suspension of this embodiment is 12.5 g / L.
[0078] Figure 2 Thermogravimetric analysis curves of antifouling agent (TCPM) and halloysite (HNTs).
[0079] Figure 3 This is a thermogravimetric analysis curve of the antifouling agent-loaded halloysite nanotubes (HNTs-TCPM) prepared in Examples 7 to 9 above.
[0080] Figure 4 It is a graph showing the antifouling agent release curve of the antifouling agent-loaded halloysite nanotubes (HNTs-TCPM) prepared in Example 8 above in water or cyclohexane.
[0081] Depend on Figure 2 , 3 It can be seen that according to the thermogravimetric curve, the antifouling agent loading amounts of the antifouling agent-loaded halloysite nanotubes prepared in Examples 7 to 9 are 1.6 wt.%, 11.6 wt.%, and 17.0 wt.%, respectively. Figure 3 It can be seen that with the increase of antifouling agent concentration, the loading rate of halloysite also increases.
[0082] Depend on Figure 4 It can be seen that the release curve of the antifouling agent (TCPM) in the antifouling agent-loaded halloysite (HNTs / TCPM) prepared in Example 8 is flat, which proves that halloysite has a slow-release effect on the release of the antifouling agent and prolongs the release time of the antifouling agent. In addition, the release rate in deionized water is slower than that in cyclohexane.
[0083] Example 10
[0084] This example is used to illustrate the preparation of halloysite nanotubes loaded with 4,5-dichloro-N-octyl-4-isothiazoline-3-one antifouling agent.
[0085] The preparation method of this embodiment is basically the same as that of embodiment 7, except that the antifouling agent used in this embodiment is 4,5-dichloro-N-octyl-4-isothiazoline-3-one, the solvent is xylene, the obtained product is abbreviated as HNTs-DCOIT, and the antifouling agent loading amount of the halloysite nanotubes is 9.8wt.%
[0086] Embodiment 11
[0087] This example is used to illustrate the preparation of halloysite nanotubes loaded with capsaicin antifouling agent.
[0088] The preparation method of this embodiment is basically the same as that of embodiment 7, except that the antifouling agent selected in this embodiment is capsaicin, the obtained product is abbreviated as HNTs-Capsaicin, and the antifouling agent loading amount of the halloysite nanotubes is 3.2 wt.%
[0089] Example 12
[0090] This example is used to illustrate the preparation of the antifouling composite material PCLU / HNTs-TCPM.
[0091] Weigh 100 parts by weight of the polycaprolactone polyurethane matrix (PCLU) prepared in Example 3 and 40 parts by weight of the antifouling agent-loaded halloysite nanotubes (HNTs-TCPM) prepared in Example 8, add them into a 150°C Haake internal mixer, blend them, take them out, and then hot-press them onto a flat plate to obtain an antifouling composite material, abbreviated as PCLU / HNTs-TCPM.
[0092] Figure 5 These are the SEM and TEM images of the antifouling composite material (PCLU / HNTs-TCPM) prepared in Example 12.
[0093] As can be seen from the figure, halloysite is well dispersed in the polycaprolactone polyurethane matrix without agglomeration, and can maintain its original tubular structure after mixing in a Haake mixer.
[0094] Embodiment 13
[0095] This example is used to illustrate the preparation of the antifouling composite material PCLU / HNTs-TCPM.
[0096] The preparation methods of this embodiment are basically the same as those of Embodiment 12, except that in this embodiment, 1 part by weight of the antifouling agent-loaded halloysite nanotube (HNTs-TCPM) raw material prepared in Embodiment 8 is weighed, and the obtained antifouling composite material is abbreviated as PCLU / HNTs-TCPM.
[0097] Embodiment 14
[0098] This example is used to illustrate the preparation of the antifouling composite material PLLAU / HNTs-DCOIT.
[0099] Weigh 100 parts by weight of the poly (L-lactide) polyurethane matrix (PLLAU) prepared in Example 5 and 60 parts by weight of the antifouling agent-loaded halloysite nanotubes (HNTs-DCOIT) prepared in Example 10, add them into a 150°C Haake internal mixer, blend them, take them out, and then hot-press them onto a flat plate to obtain an antifouling composite material, abbreviated as PLLAU / HNTs-DCOIT.
[0100] Embodiment 15
[0101] This example is used to illustrate the preparation of the antifouling composite material PPCU / HNTs-Capsaicin.
[0102] Weigh 100 parts by weight of the polypropylene carbonate polyurethane matrix (PPCU) prepared in Example 6 and 40 parts by weight of the antifouling agent-loaded halloysite nanotubes (HNTs-Capsaicin) prepared in Example 11, add them into a 150°C Haake internal mixer, blend them, take them out, and then hot-press them onto a flat plate to obtain an antifouling composite material, abbreviated as PPCU / HNTs-Capsaicin.
[0103] Comparative Example 1
[0104] This comparative example is used to illustrate the preparation of the composite material PCLU / TCPM.
[0105] The preparation method of this comparative example is basically the same as that of Example 12, except that the raw materials of this comparative example are 100 parts by weight of the polycaprolactone polyurethane matrix (PCLU) prepared in Example 3 and 4.6 parts by weight of the antifouling agent (TCPM), and the obtained composite material is abbreviated as PCLU / TCPM.
[0106] Comparative Example 2
[0107] This comparative example is used to illustrate the preparation of the composite material PCLU / HNTs.
[0108] The preparation method of this comparative example is basically the same as that of Example 12, except that the raw materials of this comparative example are 100 parts by weight of the polycaprolactone polyurethane matrix (PCLU) prepared in Example 3 and 40 parts by weight of halloysite nanotubes, and the obtained composite material is abbreviated as PCLU / HNTs.
[0109] The following is used to illustrate the performance of the antifouling agent release of the antifouling composite material:
[0110] The antifouling agent release process test was carried out on the antifouling composite material prepared in Example 12 (PCLU / / HNTs-TCPM) and the composite material prepared in Comparative Example 1 (PCLU / TCPM).
[0111] The specific steps are as follows:
[0112] Weigh 2 g of the composite material in 5 ml of deionized water, separate the solution by centrifugation at regular intervals, and add new solvent. Analyze the supernatant using UV-visible absorption spectroscopy to obtain the antifouling agent release curve, such as Figure 6 shown.
[0113] Depend on Figure 6 It can be seen that the composite material of Example 12 releases the antifouling agent more slowly than the composite material of Comparative Example 1, that is, compared with adding the antifouling agent directly to the matrix, loading the antifouling agent into halloysite can effectively prolong the release time of the antifouling agent.
[0114] The following is used to illustrate the antibacterial properties of the antifouling composite material:
[0115] Test 1:
[0116] The samples prepared in Example 12, Example 13, Comparative Example 1 and Comparative Example 2 were cut into 1 cm × 1 cm slices and suspended in the prepared culture solution of Vibrio natrii. The samples were cultured at 30°C with a rotation speed of 200 r / min for three days, and the sample surface was rinsed with PBS buffer. The sample was then placed in a 2% glutaraldehyde PBS buffer for curing for 4 hours, and finally dehydrated step by step with 60%, 70%, 80%, 90% and 99.2% ethanol solutions, and dried at low temperature. The growth of Vibrio natrii on the surface was observed by SEM, as shown in FIG. Figure 7 shown.
[0117] Test 2:
[0118] The samples prepared in Example 12 and Comparative Example 1 were cut into 1 cm × 1 cm slices and placed in 100 ml of artificial seawater prepared in advance. The rotation speed was set to 200 r / min, and mechanical stirring was performed at room temperature. The artificial seawater was replaced regularly in a cycle of 7 days, and the samples were taken out after 60 days. The same steps as in Test 1 were taken and cultured in the culture solution of Vibrio natrii for three days. The growth of Vibrio natrii on the surface of the sample was observed by SEM. Figure 8 shown.
[0119] Figure 7 These are SEM images of the sample surfaces of the composite materials prepared in Example 12, Example 13, Comparative Example 1 and Comparative Example 2 after being suspended in a culture solution of Vibrio natrii for three days.
[0120] Figure 8 These are SEM images of the sample surfaces of the composite materials prepared in Example 12 and Comparative Example 1 after being placed in artificial seawater for 60 days.
[0121] Depend on Figure 7 It can be seen that in the composite material (PCLU / HNTs-TCPM) prepared in Example 13, bacteria attached to the surface due to the small amount of HNTs-TCPM added (see Figure 7 a); The number of bacteria adhering to and growing on the surface of the composite material (PCLU / HNTs) prepared in Comparative Example 2 is relatively large, forming a layer of biofilm. This is because the added HNTs increase the surface roughness, making it easier for bacteria to settle and proliferate (see Figure 7 b); There was almost no bacterial adhesion on the surface of the composite material (PCLU / TCPM) sample prepared in Comparative Example 1 (see Figure 7 c) A small amount of bacteria adhered to the surface of the composite material (PCLU / HNTs-TCPM) sample prepared in Example 12 (see Figure 7 d), indicating that the samples prepared in Comparative Example 1 and Example 8 can inhibit bacterial attachment and prevent the formation of biofilms, and because the composite material of Comparative Example 1 releases the antifouling agent at a faster rate, the early antibacterial effect is better.
[0122] Depend on Figure 8 It can be seen that after the composite material (PCLU / TCPM) sample prepared in Comparative Example 1 was placed in seawater for 60 days, after being cultured in the culture solution of Vibrio natrii for 3 days, Vibrio natrii began to attach and proliferate on the sample surface (see Figure 8 a); No bacteria appeared on the surface of the composite material (PCLU / HNTs-TCPM) sample obtained in Example 12 (see Figure 8 b), this is because during the seawater immersion process, the TCPM molecules in the composite material (PCLU / TCPM) of Comparative Example 1 migrate to the surface at a faster rate, causing most of the TCPM to be released into the seawater, and the inhibitory effect on bacteria is weakened. Under the action of the HNTs carrier, the composite material (PCLU / HNTs-TCPM) prepared in Example 12, with the addition of HNTs-TCPM filler, can release the antifouling agent molecules into the environment at a low level and continuously, preventing the attachment of marine bacteria for a long time and improving the utilization rate of the antifouling agent.
Claims
1. An antifouling composite material, characterized in that: The antifouling composite material is prepared from raw materials including the following components: The components are calculated by weight: 100 parts by weight of polymer matrix; 1 to 100 parts by weight of sustained-release filler; The polymer matrix is a polyurethane whose main chain can be degraded into non-toxic small molecules; and the slow-release filler is a halloysite nanotube loaded with an antifouling agent.
2. The antifouling composite material according to claim 1, characterized in that: The components are calculated by weight: 100 parts by weight of polymer matrix; 1 to 60 parts by weight of sustained-release filler.
3. The antifouling composite material according to claim 1, characterized in that: The polymer matrix is one of polycaprolactone polyurethane, polylactic acid polyurethane and polycarbonate polyurethane.
4. The antifouling composite material according to claim 1, characterized in that: The polymer matrix is prepared by the following method: The polyester polyol, diisocyanate and catalyst are mixed and reacted to obtain a prepolymer, and then a chain extender is added to react to obtain a degradable polymer matrix.
5. The antifouling composite material according to claim 4, characterized in that: The polyester polyol is one of polycaprolactone diol, polypropylene carbonate diol and poly-L-lactide diol; The diisocyanate is one of isophorone diisocyanate, hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate; The catalyst is one of dimethylcyclohexylamine and dibutyltin dilaurate; The chain extender is one of 1,4-butanediol, 1,6-hexanediol and ethylene glycol.
6. The antifouling composite material according to claim 1, characterized in that: The antifouling agent is one of maleimide, isothiazolinone and capsaicin antifouling agents.
7. The antifouling composite material according to claim 1, characterized in that: The antifouling agent-loaded halloysite nanotubes are prepared by the following method: Step 1: placing the halloysite nanotubes in a muffle furnace and treating them at a high temperature of 120 to 1000° C. for 1 to 3 hours; Step 2, dissolving the antifouling agent in a solvent to prepare an antifouling agent solution with a concentration of 10 to 150 g / L; Step 3, adding the halloysite nanotubes treated in step 1 to the antifouling agent solution prepared in step 2 to prepare a suspension, and subjecting the suspension to ultrasonic dispersion treatment to make the concentration of halloysite in the suspension 5 to 300 g / L; Step 4: adopting the vacuum loading method, the suspension prepared in step 3 is stirred cyclically for 3 to 5 times under vacuum / normal pressure, and then centrifuged, washed, dried and ground to obtain the antifouling agent loaded halloysite nanotubes.
8. The antifouling composite material according to claim 7, characterized in that: In step 2, the solvent used is one of ethanol and xylene; In step 4, the vacuum pressure is -0.095 to -0.01 MPa, the rotation speed of the centrifugal separation is 5000 to 8000 r / min, and the drying temperature is 60 to 80°C.
9. A method for preparing a composite material according to any one of claims 1 to 8, characterized in that: The antifouling composite material is prepared by blending the polymer matrix and the slow-release filler in required amounts.
10. Use of the composite material according to any one of claims 1 to 8 in marine engineering equipment.
Citation Information
Patent Citations
Autocrine biomimetic anti-fouling material and application thereof
CN102977332A
Method for preparing aging-resistance rubber by utilization of halloysite slow-release anti-aging agent
CN104877178A
Antifouling composite material and preparation method thereof
CN108727675A
Long-acting sustained-release degradable antifouling polyurethane and preparation method thereof
CN109867765A
Long-acting and controllable composite anti-aging agent and preparation method and application thereof
CN112175239A