Special nylon friction-resistant injection molding material with good wear resistance for high-speed rail
By adding carbon fiber and wear-resistant components to nylon composites, the problems of poor friction performance and lack of self-lubricating performance in high-speed rail transit are solved, and the good performance of nylon friction-resistant injection molding for high-speed rail is achieved and Low cost production.
Patent Information
- Application Number
- CN202410905293.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nylon composite materials have problems such as poor friction performance and lack of self-lubricating performance in the field of high-speed rail transit, especially in low temperature environments and high production costs.
Use high-speed iron special nylon friction-resistant injection molding composed of nylon, carbon fiber, alicyclic diamine, wear-resistant, compatible agent, antioxidant, polytetrafluoroethylene, binder and dispersant, and processed through specific processes. and proportion, a material with good friction and self-lubricating properties was prepared.
It improves the wear resistance and self-lubricating properties of the material, has good stability and heat resistance, and at the same time reduces production costs, making it suitable for use in low-temperature environments.
Smart Images

Figure CN118931168A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of injection molding products, and in particular relates to a nylon friction-resistant injection molding material special for high-speed railways with good wear resistance. Background Art
[0002] Nylon is used in the field of high-speed rail transit fasteners, which can effectively solve problems such as locomotive shaking and high noise, and can ensure the stability of the wheelbase and reduce the number of maintenance times. In particular, it has good seismic resistance, which is crucial to ensure the smooth operation of railway locomotives. With the continuous increase in the speed of railway locomotives, the corresponding performance requirements for railway products are also getting higher and higher, especially in cold and frozen areas with low temperatures all year round. The fasteners (including nylon sleeves, gauge blocks, and baffle seats) on ordinary railways, high-speed railways, and subways at home and abroad all use nylon as the main raw material, which has poor low-temperature toughness, low wear resistance, and high production costs.
[0003] The Chinese patent "Research on Long Glass Fiber-Nylon Composite Materials" with application number 201610960086.1 discloses a long glass fiber-nylon composite material and a preparation method thereof, and the preparation method comprises the following steps: step 1, adding 100 parts of nylon resin; 20-30 parts of long glass fiber; 3-10 parts of toughening agent; 0.5-2 parts of flow agent; 1-2 parts of antioxidant; 2-4.5 parts of heat stabilizer into a mixer, and stirring to form a uniform first mixture; step 2, placing the first mixture in an environment with a temperature of 110-120°C and drying for 4-6 hours; adding the first mixture into a twin-screw extruder, controlling the screw speed and the temperature of the twin-screw extruder; adding 20-30 parts of long glass fiber to the screw fiber adding hole of the twin-screw extruder, melting the long glass fiber and the first mixture under the conditions of a screw speed of 35-48Hz and a temperature of 265-310°C, and mixing and extruding uniformly to obtain a long glass fiber nylon resin composition. The nylon composite material produced in this way still has the problem of poor friction performance and does not have self-lubricating properties.
[0004] To this end, the present invention provides a nylon friction-resistant injection molding material specially used for high-speed railways with good wear resistance. Summary of the invention
[0005] In view of the above problems existing in the prior art, the object of the present invention is to provide a nylon friction-resistant injection molding material specially used for high-speed railways with good wear resistance, which has the advantages of good friction performance and self-lubricating performance.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A nylon friction-resistant injection molding material for high-speed rail with good wear resistance, the raw materials are composed of the following parts by weight: 100 parts of nylon, 10-30 parts of carbon fiber, 5-12 parts of alicyclic diamine, 6-9 parts of wear-resistant material, 1-3 parts of compatibilizer, 0.1-0.3 parts of antioxidant, 5-15 parts of polytetrafluoroethylene, 2-3 parts of binder, 3-4 parts of dispersant, and 1-2 parts of light stabilizer;
[0008] The preparation process of the wear-resistant material is as follows:
[0009] (a) taking ethanol and sodium hydroxide and putting them into a mixer to mix them, then placing them in a stirrer to stir them, heating the mixture to 55-60° C. with a heater, stirring and adding tetraethyl orthosilicate dropwise, centrifuging after reaction, washing and drying to obtain material A; taking material A, polyvinyl pyrrolidone, and deionized water, mixing and dissolving them, placing them in an oil bath at 80-90° C., then adding cerium nitrate and hexamethylenetetramine, cooling and centrifuging after reaction, washing and drying, washing and drying to obtain cerium dioxide;
[0010] (b) putting urea and formaldehyde solution into a mixer, mixing and stirring with a stirrer, adjusting the pH value, heating the mixture with a heater and controlling the temperature of the mixture to be heated to 50-60° C., cooling to room temperature after the reaction, and obtaining material B;
[0011] (c) Resorcinol, ammonium chloride and sodium lignosulfonate are taken, stirred and emulsified by the stirrer, and then material B is added, the pH value is adjusted, and the reaction is carried out at 40-55° C. for 3-5 hours. After filtering and drying, the wear-resistant material is obtained.
[0012] As a preferred technical solution of the present invention, the binder includes polyvinyl alcohol.
[0013] As a preferred technical solution of the present invention, the dispersant includes sodium hexametaphosphate.
[0014] As described above, the present invention relates to a nylon friction-resistant injection molding material for high-speed rail with good wear resistance, which has the following beneficial effects:
[0015] After utilizing the above-mentioned high-speed rail special nylon friction-resistant injection molding material with good wear resistance, compared with the prior art, due to the adoption of such a structure, during the use of the nylon friction-resistant injection molding material, the polyvinyl pyrrolidone in the wear-resistant material will generate heat due to friction, and will flow out from the cerium dioxide, forming a lubricating film on the friction surface to improve the wear resistance of the product. Therefore, the present invention has the advantages of better friction performance and self-lubricating performance; and has good stability and heat resistance; and the product has low production cost and can be recycled and reused.
[0016] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a production flow chart of the wear-resistant material in the high-speed rail special nylon friction-resistant injection molding material with good wear resistance applied for by the present invention. DETAILED DESCRIPTION
[0018] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0019] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions that the present invention can be implemented, so they have no substantial technical significance. Any modification of the structure, change in the proportional relationship, or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects that the present invention can produce and the purposes that can be achieved. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. The change or adjustment of the relative relationship should also be regarded as the scope of the implementation of the present invention without substantial changes in the technical content. The specific structure can be described with reference to the drawings of the patent application.
[0020] The present invention provides a nylon friction-resistant injection molding material for high-speed railway with good wear resistance, Figure 1 As shown, the raw materials are composed of the following parts by weight: 100 parts of nylon, 10-30 parts of carbon fiber, 5-12 parts of alicyclic diamine, 6-9 parts of wear-resistant material, 1-3 parts of compatibilizer, 0.1-0.3 parts of antioxidant, 5-15 parts of polytetrafluoroethylene, 2-3 parts of binder, 3-4 parts of dispersant, and 1-2 parts of light stabilizer;
[0021] The preparation process of the wear-resistant material is as follows:
[0022] (a) taking ethanol and sodium hydroxide and putting them into a mixer to mix them, then placing them in a stirrer to stir them, heating the mixture to 55-60° C. with a heater, stirring and adding tetraethyl orthosilicate dropwise, centrifuging after reaction, washing and drying to obtain material A; taking material A, polyvinyl pyrrolidone, and deionized water, mixing and dissolving them, placing them in an oil bath at 80-90° C., then adding cerium nitrate and hexamethylenetetramine, cooling and centrifuging after reaction, washing and drying, washing and drying to obtain cerium dioxide;
[0023] (b) putting urea and formaldehyde solution into a mixer, mixing and stirring with a stirrer, adjusting the pH value, heating the mixture with a heater and controlling the temperature of the mixture to be heated to 50-60° C., cooling to room temperature after the reaction, and obtaining material B;
[0024] (c) Resorcinol, ammonium chloride and sodium lignosulfonate are taken, stirred and emulsified by the stirrer, and then material B is added, the pH value is adjusted, and the reaction is carried out at 40-55° C. for 3-5 hours. After filtering and drying, the wear-resistant material is obtained.
[0025] Example 1
[0026] (1) Weigh the raw materials according to the weight ratio: 100 parts of nylon, 20 parts of carbon fiber, 5 parts of alicyclic diamine, 6 parts of wear-resistant material, 1 part of compatibilizer, 0.2 parts of antioxidant, 5 parts of polytetrafluoroethylene, 2 parts of binder, 3 parts of dispersant, and 1 part of light stabilizer;
[0027] (2) irradiating 5 parts of the prepared polytetrafluoroethylene with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 1 hour, and irradiating 20 parts of the prepared carbon fiber with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 2 hours;
[0028] (3) adding 100 parts of dried nylon 6 pellets and the high-density polyethylene obtained in step (2), 5 parts of polytetrafluoroethylene (PTFE) ultrafine powder, 0.2 parts of antioxidant, 1 part of compatibilizer CMG9805, 1 part of light stabilizer, and 6 parts of wear-resistant material, and stirring and mixing them evenly in a high-speed mixer;
[0029] (4) feeding the material obtained in step (3) into a twin-screw extruder through a feeder, and adding the carbon fiber obtained in step (2) to the side feeding port of the twin-screw extruder, wherein the temperature of each section of the twin-screw extruder from the feeding port to the die head is 180° C., 200° C., 230° C., and 210° C., respectively, and the rotation speed is 180 rpm;
[0030] (5) The material obtained in step (4) is subjected to strip drawing, cooling, pelletizing and drying treatments, and then injection molded on an injection molding machine to obtain an injection molding material, see Table 1.
[0031] Example 2
[0032] (1) Weigh the raw materials according to the weight ratio: 100 parts of nylon, 10 parts of carbon fiber, 12 parts of alicyclic diamine, 6 parts of wear-resistant material, 1 part of compatibilizer, 0.1 part of antioxidant, 15 parts of polytetrafluoroethylene, 3 parts of binder, 4 parts of dispersant, and 2 parts of light stabilizer;
[0033] (2) irradiating 5 parts of the prepared polytetrafluoroethylene with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 3 hours, and irradiating 20 parts of the prepared carbon fiber with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 1.5 hours;
[0034] (3) adding 15 parts of polytetrafluoroethylene (PTFE) ultrafine powder, 0.1 parts of antioxidant, 1 part of compatibilizer CMG9805, 2 parts of light stabilizer, and 6 parts of wear-resistant material to 100 parts of dried nylon 6 pellets and the high-density polyethylene obtained in step (2), and stirring and mixing them evenly in a high-speed mixer;
[0035] (4) feeding the material obtained in step (3) into a twin-screw extruder through a feeder, and adding the carbon fiber obtained in step (2) to the side feeding port of the twin-screw extruder, wherein the temperature of each section of the twin-screw extruder from the feeding port to the die head is 180° C., 200° C., 230° C., and 210° C., respectively, and the rotation speed is 180 rpm;
[0036] (5) The material obtained in step (4) is subjected to strip drawing, cooling, pelletizing and drying treatments, and then injection molded on an injection molding machine to obtain an injection molding material, see Table 1.
[0037] Comparative Example 1:
[0038] (1) Weigh the raw materials according to the weight ratio: 100 parts of nylon, 20 parts of carbon fiber, 5 parts of alicyclic diamine, 1 part of compatibilizer, 0.2 parts of antioxidant, 5 parts of polytetrafluoroethylene, 2 parts of binder, 3 parts of dispersant, and 1 part of light stabilizer;
[0039] (2) irradiating 5 parts of the prepared polytetrafluoroethylene with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 1 hour, and irradiating 20 parts of the prepared carbon fiber with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 2 hours;
[0040] (3) adding 100 parts of dried nylon 6 pellets and the high-density polyethylene obtained in step (2), 5 parts of polytetrafluoroethylene (PTFE) ultrafine powder, 0.2 parts of antioxidant, 1 part of compatibilizer CMG9805, and 1 part of light stabilizer, and stirring and mixing them evenly in a high-speed mixer;
[0041] (4) feeding the material obtained in step (3) into a twin-screw extruder through a feeder, and adding the carbon fiber obtained in step (2) to the side feeding port of the twin-screw extruder, wherein the temperature of each section of the twin-screw extruder from the feeding port to the die head is 180° C., 200° C., 230° C., and 210° C., respectively, and the rotation speed is 180 rpm;
[0042] (5) The material obtained in step (4) is subjected to strip drawing, cooling, pelletizing and drying treatments, and then injection molded on an injection molding machine to obtain an injection molding material, see Table 1.
[0043] Comparative Example 2:
[0044] (1) Weigh the raw materials according to the weight ratio: 100 parts of nylon, 10 parts of carbon fiber, 12 parts of alicyclic diamine, 1 part of compatibilizer, 0.1 part of antioxidant, 15 parts of polytetrafluoroethylene, 3 parts of binder, 4 parts of dispersant, and 2 parts of light stabilizer;
[0045] (2) irradiating 5 parts of the prepared polytetrafluoroethylene with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 3 hours, and irradiating 20 parts of the prepared carbon fiber with 60Coγ-rays or an electron accelerator at a dose rate of 8kGy / h for 1.5 hours;
[0046] (3) adding 15 parts of polytetrafluoroethylene (PTFE) ultrafine powder, 0.1 parts of antioxidant, 1 part of compatibilizer CMG9805, and 2 parts of light stabilizer to 100 parts of dried nylon 6 pellets and the high-density polyethylene obtained in step (2), and stirring and mixing the mixture in a high-speed mixer;
[0047] (4) feeding the material obtained in step (3) into a twin-screw extruder through a feeder, and adding the carbon fiber obtained in step (2) to the side feeding port of the twin-screw extruder, wherein the temperature of each section of the twin-screw extruder from the feeding port to the die head is 180° C., 200° C., 230° C., and 210° C., respectively, and the rotation speed is 180 rpm;
[0048] (5) The material obtained in step (4) is subjected to strip drawing, cooling, pelletizing and drying treatments, and then injection molded on an injection molding machine to obtain an injection molding material, see Table 1.
[0049] Table 1 is the test results of the main performance indicators of the friction-resistant injection molding material applied in the present invention
[0050] Test items Example 1 Example 2 Comparative Example 1 Comparative Example 2 Tensile Strength 100.2 112.2 132.3 99.7 Friction coefficient 0.112 0.114 0.103 0.131 Friction torque 380.2 393.4 375.4 403.1
[0051] It can be seen from this that the comprehensive performance of the nylon friction-resistant injection molding material prepared by the method of the present invention is better than that of the comparative example.
[0052] In this embodiment, the binder includes polyvinyl alcohol.
[0053] In this embodiment, the dispersant includes sodium hexametaphosphate.
[0054] As described above, the present invention relates to a nylon friction-resistant injection molding material for high-speed rail with good wear resistance, which has the following beneficial effects:
[0055] After utilizing the above-mentioned high-speed rail special nylon friction-resistant injection molding material with good wear resistance, compared with the prior art, due to the adoption of such a structure, during the use of the nylon friction-resistant injection molding material, the polyvinyl pyrrolidone in the wear-resistant material will generate heat due to friction, and will flow out from the cerium dioxide, forming a lubricating film on the friction surface to improve the wear resistance of the product. Therefore, the present invention has the advantages of better friction performance and self-lubricating performance; and has good stability and heat resistance; and the product has low production cost and can be recycled and reused.
[0056] In summary, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.
[0057] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A nylon friction-resistant injection molding material for high-speed rail with good wear resistance. It is characterized in that The raw materials are composed of the following parts by weight Composition: 100 parts of nylon, 10-30 parts of carbon fiber, 5-12 parts of alicyclic diamine, 6-9 parts of wear-resistant material, 1-3 parts of compatibilizer, 0.1-0.3 parts of antioxidant, 5-15 parts of polytetrafluoroethylene, 2-3 parts of binder, 3-4 parts of dispersant, 1-2 parts of light stabilizer; The preparation process of the wear-resistant material is as follows: (a) taking ethanol and sodium hydroxide and putting them into a mixer to mix them, then placing them in a stirrer to stir them, heating the mixture to 55-60° C. with a heater, stirring and adding tetraethyl orthosilicate dropwise, centrifuging after reaction, washing and drying to obtain material A; taking material A, polyvinyl pyrrolidone and deionized water and dissolving them, placing them in an oil bath at 80-90° C., then adding cerium nitrate and hexamethylenetetramine, cooling and centrifuging after reaction, washing and drying, washing and drying to obtain cerium dioxide; (b) putting urea and formaldehyde solution into a mixer, mixing and stirring with a stirrer, adjusting the pH value, heating the cerium dioxide in (a) with a heater to obtain a mixture and controlling the temperature of the mixture to be heated to 50-60° C., cooling to room temperature after the reaction, and obtaining material B; (c) Resorcinol, ammonium chloride and sodium lignosulfonate are taken, stirred and emulsified by the stirrer, and then material B is added, the pH value is adjusted, and the reaction is carried out at 40-55° C. for 3-5 hours. After filtering and drying, the wear-resistant material is obtained.
2. A nylon friction-resistant injection molding material for high-speed rail with good wear resistance as claimed in claim 1, Features: The binder includes polyvinyl alcohol.
3. The nylon friction-resistant injection molding material for high-speed rail with good wear resistance as claimed in claim 1, Features: The dispersant includes sodium hexametaphosphate.