Polyamide powder not easy to carry static electricity and preparation method thereof

By adding surface charge modifiers and positive charge flow aids to the polyamide powder, the problems of dust and powder barrel wall accumulation caused by static electricity in the fluidized bed immersion process are solved, and the fluidity and immersion effect are improved , reduces the risk of deflagration and improves coating performance.

CN118931174APending Publication Date: 2024-11-12ORINKO HIGH PERFORMANCE MATERIALS TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411063380.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Polyamide powder is prone to accumulation of dust and powder barrel walls due to electrostatic effects in the fluidized bed dip process, which affects utilization and fluidization effects, and may cause explosion risks. The existing antistatic measures affect the coating performance and physical and chemical properties. Performance risks.

Method used

The pH value of the polyamide powder is reduced by adding a surface charge modifier, making the surface positively charged, and combined with a positive charge flow additive, it can jointly improve the charge condition of the powder, reduce static aggregation, improve fluidity and immersion effect.

Benefits of technology

It effectively reduces the electrostatic accumulation of powder, improves fluidity and dip effect, reduces dust and powder barrel wall accumulation, reduces the risk of deflagration, and improves the appearance and feel of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978655120000061
    Figure BDA0004978655120000061
Patent Text Reader

Abstract

The invention relates to polyamide powder not easy to carry static electricity and a preparation method thereof. The polyamide powder not easy to carry static electricity is prepared from the following components in parts by weight: 100 parts of polyamide powder, 0-2 parts of an interference material, 0-2 parts of toner, 0.01-0.2 part of a surface charge modifier and 0.01-0.3 part of a positive charge flow promoter. The pH value of the surface of the polyamide powder is reduced to a polyamide isoelectric point (Ip = 5-6) by adding the surface charge modifier, so that the surface of the polyamide powder is positively charged, and the charged condition of the surface of the polyamide powder is further improved by further adding the positively charged flow promoter; due to the fact that the flowability of the polyamide powder is usually reduced due to the addition of the surface charge modifier, the added flow promoter with positive charges can achieve a synergistic effect on surface charges of the polyamide powder and the charge modifier, and the adverse effect of the charge modifier on the flowability of the powder can be overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a polyamide powder that is not prone to static electricity and a preparation method thereof. Background Art

[0002] Fluidized bed dipping process is a process in which powder is fluidized in a fluidized bed, and then the workpiece is immersed in it. The powder then adheres to the surface of the workpiece due to temperature or other effects, thereby forming a coating. Among them, polyamide powder is a material that is often used in this process for surface coating of metal materials. This material can be used in a variety of applications such as dishwasher baskets, springs, bearings, etc. that require water resistance, heat resistance, aging resistance, or a low friction coefficient.

[0003] However, in actual use, due to the small particle size of polyamide powder and the repeated friction between powders during fluidization, and due to the high resistance of nylon, the surface of polyamide powder usually accumulates more charges and cannot dissipate. Usually, dust is carried away by the suction device or accumulated on the wall of the fluidization barrel, affecting the utilization rate of polyamide powder. Polyamide powder is sometimes too charged, affecting the fluidization effect and the dipping effect. Since the dipping process uses gas or other heating furnaces, if the dust is too large, it may also cause risks such as deflagration or even explosion, and excessive dust also poses a risk to the health of on-site operators.

[0004] If no liquid is added to the polyamide powder to attach the color powder to the powder surface, the probability of dust generation is higher due to the smaller particle size of the color powder and interference material used for color adjustment, which is sucked away by the dust collection device. After long-term use, the color will change due to the reduction of color powder and interference material; or the enriched color powder on the barrel wall will fall and form color blocks or color spots on the workpiece surface. You can also choose to use liquid to attach the color powder to the surface of the polyamide powder, but on the one hand, the liquid will reduce the fluidity of the powder and make it difficult for the powder to fluidize; on the other hand, improper selection of liquid will also affect the appearance and feel of the coating surface.

[0005] The method of improving the dust caused by static electricity usually involves adding antistatic components to the polyamide powder internally or externally. The internal antistatic component is added by adding conductive components to the powder resin to reduce the resistance value of the powder itself to 10 9Ω / cm or less, which requires filling a large amount (usually >2%) of conductive materials or additives, and the resin needs to be re-extruded and modified. The changes in physical and chemical properties brought about by this process may affect subsequent use. The external addition of antistatic ingredients is relatively simple, that is, directly mixing antistatic agents in the powder, which can not only make the color powder adhere to the powder surface, but also reduce the static electricity generated by the powder and enrichment on the barrel wall, thereby reducing defects during dipping. Since powders usually carry negative charges, conventional antistatic agents are mostly cationic surfactants, but most cationic surfactants have a low decomposition temperature, and are very likely to produce defects such as fish eyes and foaming during dipping. Summary of the invention

[0006] Based on this, the purpose of the present invention is to provide a polyamide powder that is not easy to carry static electricity and a preparation method thereof, by adjusting the charge on the surface of the polyamide powder, reducing the level of static electricity accumulation on the surface of the polyamide powder, reducing the shortcomings such as dust and powder barrel wall accumulation during dipping, and improving the powder fluidity and dipping effect.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] The invention provides a polyamide powder which is not easy to be charged with static electricity. The polyamide powder is prepared from the following components in parts by weight: 100 parts of polyamide powder, 0-2 parts of interference material, 0-2 parts of color powder, 0.01-0.2 parts of surface charge modifier, and 0.01-0.3 parts of positive charge flow aid.

[0009] The present invention reduces the surface pH value of polyamide powder to the isoelectric point of polyamide (Ip=5-6) by adding a surface charge modifier, so that the surface of the polyamide powder is positively charged, and further adds a positively charged flow aid to further improve the charging condition of the surface of the polyamide powder. Since the addition of the surface charge modifier usually reduces the fluidity of the polyamide powder, the addition of the positively charged flow aid can not only play a synergistic role with the charge modifier on the surface charge of the polyamide powder, but also overcome the adverse effect of the charge modifier on the powder fluidity.

[0010] As a further improvement of the above solution of the present invention, the surface charge modifier is an aqueous solution of an acidic substance.

[0011] As a further improvement of the above solution of the present invention, the concentration of the aqueous solution of the acidic substance is 0.1-10%;

[0012] And / or, the dissociation constant pKa value of the acidic substance is between 3-6.

[0013] As a further improvement of the above solution of the present invention, the positive charge flow aid is an inorganic powder with an isoelectric point Ip value greater than 7.

[0014] As a further improvement of the above solution of the present invention, the particle size D50 of the inorganic powder is less than 500 nm.

[0015] As a further improvement of the above-mentioned scheme of the present invention, the polyamide powder is a blend / copolymer of one or more of PA11, PA12, PA610, PA612, PA510, PA513, PA515, PA1012, PA1212, PA1010, PA6, PA66, PA46, PA56 and nylon elastomer.

[0016] As a further improvement of the above solution of the present invention, the polyamide powder has a melt index of less than 60 g / 10 min and a particle size of 10-300 μm.

[0017] As a further improvement of the above solution of the present invention, the interference material is any one of mica powder, glass flakes, and ultrafine metal powder, wherein the mica powder and the glass flakes have a coating or a deposition layer.

[0018] As a further improvement of the above solution of the present invention, the toner is an inorganic powder with color covering property.

[0019] The present invention provides a method for preparing the polyamide powder that is not easy to be charged with static electricity as described above, comprising the following steps: putting polyamide powder and surface charge modifier into a high-speed mixer in proportion and continuously stirring at 600-1000 rpm for 3-10 minutes, then adding interference material, color powder and positive charge flow aid in proportion and continuously stirring at 600-1000 rpm for 3-10 minutes to obtain the polyamide powder that is not easy to be charged with static electricity.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention reduces the surface pH value of polyamide powder to the isoelectric point of polyamide (Ip=5-6) by adding a surface charge modifier, so that the surface of the polyamide powder is positively charged, and further adds a positively charged flow aid to further improve the charging condition of the surface of the polyamide powder. Since the addition of the surface charge modifier usually reduces the fluidity of the polyamide powder, the addition of the positively charged flow aid can not only play a synergistic role with the charge modifier on the surface charge of the polyamide powder, but also overcome the adverse effect of the charge modifier on the powder fluidity. DETAILED DESCRIPTION

[0022] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0024] The specific information of the raw materials used in the following examples and comparative examples is as follows:

[0025] Polyamide powder: PA612 from Shandong Dongchen Ruisen, with surface resistance >10 11 Ω; The polyamide particles are cooled to below -100°C in liquid nitrogen and ground into powder by mechanical crushing, and then a powder with a particle size of 10-300 μm is sieved with a suitable sieve, and the melt index is 30 g / 10 min;

[0026] Interference material: mica powder, Iriodin 6111, Merck;

[0027] Toner: Iron black, BAYFERROX 318M, LANXESS;

[0028] Surface charge modifier 1: sodium dihydrogen citrate, Wokai, pKa2 = 4.76;

[0029] Surface charge modifier 2: dilute sulfuric acid, 10% solution, pKa = -3;

[0030] Positive charge flow aid: fumed alumina, Alu C, Ip = 7-8, Evonik;

[0031] Negatively charged flow aid: fumed silica, Areosol A200, Ip≈2, Evonik.

[0032] All the above materials are commercially available conventional products.

[0033] It is to be understood that the above raw materials and reagents are only examples of some specific embodiments of the present invention, so that the technical solution of the present invention is clearer, and it does not mean that the present invention can only use the above reagents, and the specific scope in the claims shall prevail. In addition, the "parts" described in the examples and comparative examples, unless otherwise specified, refer to parts by weight.

[0034] Any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0035] Example 1

[0036] This embodiment provides a polyamide powder that is not prone to static electricity, which is prepared from the following components in parts by weight: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, 0.1 parts of surface charge modifier 1, and 0.1 parts of positive charge flow aid.

[0037] The preparation method of the polyamide powder that is not easy to be charged with static electricity in this embodiment comprises the following steps: polyamide powder and surface charge modifier 1 are put into a high-speed mixer in proportion and stirred continuously at 600-1000 rpm for 3-10 minutes, and then interference material, color powder and positive charge flow aid 1 are added in proportion and stirred continuously at 600-1000 rpm for 3-10 minutes to obtain polyamide powder that is not easy to be charged with static electricity.

[0038] Example 2

[0039] This embodiment adopts the same implementation method as Example 1, and the difference from Example 1 is that the weight parts of each component in this embodiment are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, 0.2 parts of surface charge modifier 1, and 0.3 parts of positive charge flow aid.

[0040] Example 3

[0041] This embodiment adopts the same implementation method as Example 1, and the difference from Example 1 is that the weight parts of each component in this embodiment are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, 0.01 parts of surface charge modifier 1, and 0.01 parts of positive charge flow aid.

[0042] Comparative Example 1

[0043] This comparative example adopts the same implementation method as Example 1, and the difference from Example 1 is that the weight parts of each component in this comparative example are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, 0.1 parts of surface charge modifier 2, and 0.1 parts of positive charge flow aid.

[0044] Comparative Example 2

[0045] This comparative example adopts the same implementation as Example 1, and the difference from Example 1 is that the weight parts of each component in this comparative example are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, and 0.2 parts of surface charge modifier 1.

[0046] Comparative Example 3

[0047] This comparative example adopts the same implementation method as Example 1, and the difference from Example 1 is that the weight parts of each component in this comparative example are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, 0.01 parts of surface charge modifier 1, and 0.01 parts of negative charge flow aid.

[0048] Comparative Example 4

[0049] This comparative example adopts the same implementation as Example 1, and the difference from Example 1 is that the weight parts of each component in this comparative example are: 100 parts of polyamide powder, 0.5 parts of interference material, 0.2 parts of color powder, and 0.3 parts of positive charge flow aid.

[0050] The amounts of the components in the above examples and comparative examples are shown in Table 1.

[0051] Table 1 Amount of each component in the examples and comparative examples (parts by weight)

[0052]

[0053] Test Case

[0054] The performance of the polyamide powders obtained in Examples 1-3 and Comparative Examples 1-4 was tested in the following manner:

[0055] a. Powder fluidity: tested according to GB / T 31057.3-2018 method, expressed by the powder repose angle. The smaller the repose angle, the better the fluidity.

[0056] b. Powder dust level: Use a fluidizing barrel with a diameter of 25 cm and a height of 50 cm, load 1.5 kg of powder product, install an air suction filter device on the top of the fluidizing barrel under 30 L / min compressed air, and test the dust quality of the powder after fluidization;

[0057] c. Powder accumulation on the wall: After fluidization for 2 hours according to the method in b, carefully pour out the powder in the fluidized barrel, and try not to touch the powder hanging on the wall during the process. Then test the mass difference of the fluidized barrel before and after fluidization, which is the mass of the powder hanging on the wall.

[0058] d. Powder aging resistance: Heat a 2mm thick steel plate to 400℃, then dip-coat the powder on the surface of the steel plate, and then age it in an oven at 110℃ for one week. Test the coating toughness when the steel plate is bent 90° on a steel pipe with a radius of 1cm.

[0059] The above performance test results are shown in Table 2.

[0060] Table 2 Performance test results

[0061] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Flowability / angle of repose 34° 31° 36° 35° 45° 36° 30° Dust / quality 0.4g 0.2g 1.3g 0.3g 1.0g 3.4g 3.2g Wall powder accumulation / mass 2g 3g 4g 1g 3g 10g 1g Powder aging resistance Uncracked Uncracked Uncracked Cracking Uncracked Uncracked Uncracked

[0062] Combined with Table 1-2 for analysis:

[0063] From the comparison between Comparative Example 1 and Example 1, it can be seen that the combination of surface charge modifier 1 and positive charge flow aid has better fluidity, dust suppression and wall accumulation prevention effects; while the use of surface charge modifier 2 with too strong acidity will have an adverse effect on the resin during the aging process, resulting in the coating being more prone to cracking after aging.

[0064] By comparing Comparative Example 2 with Example 2, it can be seen that if only surface charge modifier 1 is used without the positive charge flow aid, the fluidity of the powder will be significantly reduced, resulting in fluidization difficulties and the formation of more fluidization defects such as "rat holes", from which dust is more easily ejected, resulting in slightly higher dust emission.

[0065] By comparing Comparative Example 3 and Example 3, it can be seen that: since the negatively charged flow aid is negatively charged, which is opposite to the charge of the positively charged flow aid, there is no significant difference between the two in the initial process. However, after long-term fluidization to generate static electricity, the dust and wall accumulation are significantly worse than the positively charged flow aid.

[0066] Comparison between Comparative Example 4 and Example 2 shows that: using only the positively charged flow aid has better fluidity and does not produce wall accumulation, but lacks liquid to bind the interference material and color powder to the surface of the polyamide powder, so more dust is still generated.

[0067] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0068] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A polyamide powder that is not prone to static electricity, characterized in that: The invention is prepared from the following components in parts by weight: 100 parts of polyamide powder, 0-2 parts of interference material, 0-2 parts of color powder, 0.01-0.2 parts of surface charge modifier and 0.01-0.3 parts of positive charge flow aid.

2. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The surface charge modifier is an aqueous solution of an acidic substance.

3. The polyamide powder that is not prone to static electricity according to claim 2, characterized in that The aqueous solution concentration of the acidic substance is 0.1-10%; And / or, the dissociation constant pKa value of the acidic substance is between 3-6.

4. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The positive charge flow aid is an inorganic powder with an isoelectric point Ip value greater than 7.

5. The polyamide powder that is not prone to static electricity according to claim 4, characterized in that The particle size D50 of the inorganic powder is less than 500 nm.

6. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The polyamide powder is a blend / copolymer of one or more of PA11, PA12, PA610, PA612, PA510, PA513, PA515, PA1012, PA1212, PA1010, PA6, PA66, PA46, PA56 and nylon elastomer.

7. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The polyamide powder has a melt index of less than 60 g / 10 min and a particle size of 10-300 μm.

8. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The interference material is any one of mica powder, glass flakes, and ultrafine metal powder, wherein the mica powder and the glass flakes have a coating or a deposition layer.

9. The polyamide powder that is not prone to static electricity according to claim 1, characterized in that The toner is an inorganic powder with color hiding properties.

10. A method for preparing a polyamide powder that is not prone to static electricity according to any one of claims 1 to 9, characterized in that: The following steps are involved: Put polyamide powder and surface charge modifier into a high-speed mixer in proportion and stir continuously for 3-10 minutes at 600-1000 rpm, then add interference material, color powder and positive charge flow aid in proportion and stir continuously for 3-10 minutes at 600-1000 rpm to obtain polyamide powder that is not easy to carry static electricity.

Citation Information

Patent Citations

  • PA66 / PA6 (Polyamide 66 / Polyamide 6) copolymerized material for selective laser sintering and preparation method

    CN106977711A

  • Antistatic polymide powder material for selective laser sintering and preparation method of antistatic polymide powder material

    CN107236288A

  • Flowing powder hot-melt adhesive and preparation method thereof

    CN107384251A

  • Polyamide composition and preparation method thereof

    CN115160779A

  • Polyamide powder coating for metal surface coating and preparation method thereof

    CN115260895A