High-hardness gun-mixing type dental occlusion recording silicone rubber and preparation method thereof
The hardness in the prior art is solved by using a combination of linear vinyl silicone oil, branched vinyl silicone oil, hydrogen-containing silicone oil, vinyl MQ silicone resin, nanofiller and reinforced filler of a specific proportion in dental occlusal recording materials. With the problem of difficulty in balancing consistency, high-precision occlusal recording materials with high hardness and low consistency are achieved, suitable for dental mixing guns.
Patent Information
- Application Number
- CN202411155949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing dental occlusal recording materials are difficult to meet the requirements of low consistency while increasing their hardness, which affects the mixing and use of materials, especially when mixing through mixing guns in clinical practice.
10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogen-containing silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nanofiller, 20- A combination of 55% reinforced filler, 0.1% to 2% platinum catalyst, 0.5~5% plasticizer, vacuum degassing through a kneader, and prepare high-hardness gun mixed bite recording silicone rubber to ensure high hardness and suitable material Consistency.
It achieves a balance of high hardness and low consistency, suitable for dental mixing guns. After mixing and curing, Shore A has a hardness of up to 95, and the consistency is suitable, suitable for obtaining high-precision dental occlusal recording impressions.
Smart Images

Figure BDA0005004977910000091 
Figure BDA0005004977910000092 
Figure BDA0005004977910000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dental occlusal relationship recording materials, and in particular relates to a gun-mixed dental occlusal recording silicone rubber with high hardness and a preparation method thereof. Background Art
[0002] Bite registration is one of the key factors in making accurate and high-quality restorations. Bite registration has the following functions: providing accurate jaw relationship; avoiding misalignment of the occlusal contact point, causing pain or damage to the temporomandibular joint; avoiding excessive adjustment of the restoration or the opposing teeth due to occlusal problems. Incorrect occlusal relationship may cause long-term headaches, fractured jaw joints, inability to open or close the mouth freely, pain when chewing, neck and throat pain, jaw joint fatigue, eye pain, difficulty swallowing and other problems.
[0003] Commonly used bite record materials in clinic include bite wax, silicone rubber weight, and resin type materials. The above materials have obvious disadvantages. Among them, bite wax has large polymerization shrinkage and is easy to deform and break; silicone rubber weight takes a long time to polymerize, and is elastic after curing, which will cause certain deviations; and resin type materials take a long time to polymerize, are complicated to operate, are not suitable for long dentition, and have large shrinkage.
[0004] Bite recording silicone rubber is an addition-type room temperature vulcanized silicone rubber, which is generally composed of two components: a matrix and a catalyst. The two components are mixed when used, and the vinyl in the vinyl silicone oil and the silicon-hydrogen bonds in the hydrogen-containing silicone oil are cross-linked and polymerized under the action of a platinum catalyst. It can be used specifically to record dental occlusal relationships. Compared with other bite recording materials, it has the advantages of easy use, suitable operation time, good dimensional contour stability (not sensitive to heat), high impression accuracy, no resistance during occlusion, sterilization, and long-term storage.
[0005] In actual use, the bite record material is generally required to have both high hardness and low consistency. The high hardness of the material can prevent the material from being compressed and deformed due to external forces, making the recorded occlusal relationship more precise, and it is not affected by compression or bending during resetting, which facilitates the subsequent preparation of precise restorations. In addition, the material consists of two components, a matrix and a catalyst, which need to be mixed during clinical use. The appropriate consistency can ensure that the material can be extruded by a dental mixing gun and then mixed through a mixing tube. The material mixed by this method is free of bubbles and is easier to operate clinically.
[0006] In the prior art, suitable vinyl silicone oil, crosslinking agent, etc. are generally selected to increase the crosslinking density, thereby increasing the hardness of the material. In addition, the filler content can also be increased to increase the hardness of the material, but increasing the filler content will also increase the consistency of the material, which is not conducive to mixing through a mixing gun and a mixing tube during clinical use. For example, patent CN 115804720 A discloses a dental silicone rubber bite recording material, which uses flaky powder as a filler to prepare a high-hardness bite recording material, but its consistency value is less than 30mm. The smaller the consistency value, the greater the consistency, which is not suitable for mixing with a mixing gun in clinical use. Summary of the invention
[0007] In view of one or more of the above defects or improvement needs in the prior art, the present invention provides a high-hardness gun-mixed dental bite registration silicone rubber and a preparation method thereof, which can improve the hardness of the silicone rubber while meeting the consistency requirements.
[0008] To achieve the above object, according to one aspect of the present invention, a high-hardness gun-mixed bite-recording silicone rubber is provided, wherein the raw materials thereof include, by weight percentage:
[0009] 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogen-containing silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst, 0.5-5% plasticizer.
[0010] As a further improvement of the present invention, the linear vinyl silicone oil is methyl vinyl polysiloxane or methyl phenyl vinyl polysiloxane with vinyl groups at both ends of the molecular chain, and one molecule thereof contains 2 vinyl groups; and / or,
[0011] The branched vinyl silicone oil is a methyl vinyl polysiloxane having vinyl groups at both ends and in the middle of the molecular chain, and one molecule thereof contains at least 3 vinyl groups; and / or,
[0012] The hydrogen-containing silicone oil is a methyl polysiloxane containing a Si-H group in the middle of the molecular chain.
[0013] As a further improvement of the present invention, the matrix system and the catalyst system are included; in terms of weight percentage,
[0014] The matrix system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogenated silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, and 0.5-5% plasticizer;
[0015] The catalyst system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst and 0.5-5% plasticizer.
[0016] As a further improvement of the present invention,
[0017] The chemical formula of the linear vinyl silicone oil is:
[0018] (CH2=CH2)(CH3)2SiO[RR'SiO] m [R'R"SiO] n Si(CH3)2(CH2=CH2), wherein R is CH3 or C6H5, R' is CH3 or C6H5, and R" is CH3 or C6H5;
[0019] and / or,
[0020] The chemical formula of the branched vinyl silicone oil is:
[0021] (CH2=CH)(CH3)2SiO[(CH3)2SiO] m [(CH2=CH)CH3SiO] n Si(CH3)2(CH2=CH);
[0022] and / or,
[0023] The general chemical formula of the hydrogen-containing silicone oil is:
[0024] (CH3)3SiO[RR'SiO] m [R'R"SiO] n Si(CH3)3, wherein R is H, R' is H or CH3, and R" is H or CH3.
[0025] As a further improvement of the present invention, the linear vinyl silicone oil includes at least two materials with different viscosities; the viscosity range of the low viscosity material is 10 to 100 cst, and the viscosity range of the medium viscosity material is 200 to 1000 cst; preferably, the viscosity range of the low viscosity material is 20 to 50 cst, and the viscosity range of the medium viscosity material is 250 to 400 cst.
[0026] As a further improvement of the present invention, in the linear vinyl silicone oil, the mass ratio of the low-viscosity material to the medium-viscosity material is 1:0.5-2.0, preferably 1:0.8-1.2.
[0027] As a further improvement of the present invention, the general chemical formula of the vinyl MQ silicone resin is:
[0028] (CH3)2(CH2=CH)SiO 1 / 2 ] a [(CH3)3SiO 1 / 2 ] b [SiO 4 / 2 ] c
[0029] Among them [(CH3)2(CH2=CH)SiO 1 / 2 ] a [(CH3)3SiO 1 / 2 ] b is the M group, [SiO 4 / 2 ] c is a Q group;
[0030] Preferably, the molar ratio of the M group to the Q group is 0.6 to 1.0.
[0031] As a further improvement of the present invention,
[0032] The hydrogen content of the hydrogen-containing silicone oil is 0.6-1.5%; and / or,
[0033] The vinyl MQ silicone resin has a vinyl content of 1 to 3%.
[0034] As a further improvement of the present invention,
[0035] The nanofiller is hydrophobically treated nano-silicon dioxide and / or nano-alumina powder, preferably, the average particle size of the nanofiller is 5 to 100 nm; and / or,
[0036] The reinforcing filler is hydrophobically treated silica and / or alumina powder, preferably, the average particle size of the reinforcing filler is 5 to 100 μm; and / or,
[0037] The platinum catalyst is a Custer catalyst with a platinum content of 1% to 2%; and / or,
[0038] The plasticizer is liquid paraffin and / or white vaseline.
[0039] According to another aspect of the present invention, there is provided a method for preparing the high-hardness gun-mixed bite-registering silicone rubber, comprising the following steps:
[0040] Weigh the materials of the matrix system, mix them in a kneader, and then vacuum degas to prepare the matrix system; the matrix system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogenated silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, and 0.5-5% plasticizer;
[0041] The materials of the catalyst system are weighed, mixed by a kneader, and then vacuum degassed to prepare a catalyst system; the catalyst system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst, and 0.5-5% plasticizer;
[0042] The matrix system and the catalyst system are respectively filled into a two-component rubber cartridge.
[0043] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:
[0044] (1) The high-hardness gun-mixed dental occlusal recording silicone rubber of the present invention has good toughness through the synergistic effect of low-viscosity and medium-viscosity materials in the straight-chain vinyl silicone oil, and does not affect its hardness. The branched vinyl silicone oil and the high-hydrogen content vinyl silicone oil can provide more cross-linking points for the material, providing a good foundation for the overall high hardness and low viscosity. The vinyl MQ silicone resin further plays a reinforcing role, which can improve the hardness of the silicone rubber while meeting the consistency requirements, and is suitable for mixing with a mixing gun.
[0045] (2) The high-hardness gun-mixed dental bite-recording silicone rubber of the present invention can further improve the hardness of the product through the combined action of nanofillers and reinforcing fillers of different particle sizes, while not making the product too thick.
[0046] (3) The high-hardness gun-mixed dental bite registration silicone rubber of the present invention has a Shore A hardness of up to 95 after mixing and curing, and has a suitable consistency (consistency value greater than 35 mm), and has the advantages of high impression accuracy and dimensional stability. It is particularly suitable for obtaining high-precision dental bite registration impressions. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0048] The present invention provides a high-hardness silicone rubber for dental bite registration that has the advantages of general silicone rubber, and can meet the consistency requirements while improving the hardness of the material. It is suitable for mixing with a mixing gun and can be easily extruded and mixed evenly by a dental mixing gun. As a preferred embodiment, the high-hardness gun-mixed bite registration silicone rubber of the embodiment of the present invention includes, by weight percentage, the raw materials:
[0049] 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogen-containing silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst, 0.5-5% plasticizer.
[0050] In a preferred embodiment, the linear vinyl silicone oil is a methyl vinyl polysiloxane with vinyl groups at both ends of the molecular chain, wherein the methyl group may also be substituted by a phenyl group, etc., and one molecule contains two vinyl groups. Preferably, the chemical formula of the linear vinyl silicone oil is:
[0051] (CH2=CH2)(CH3)2SiO[RR'SiO] m [R'R"SiO] n Si(CH3)2(CH2=CH2), wherein R is CH3 or C6H5, R' is CH3 or C6H5, and R" is CH3 or C6H5.
[0052] The linear vinyl silicone oil is composed of at least two materials with different viscosities, one is a low-viscosity material with a viscosity range of 10cst to 100cst, more preferably 20 to 50cst; the other is a medium-viscosity material with a viscosity range of 200 to 1000cst, more preferably 250 to 400cst. Its specific viscosity is determined by the values of m and n in the chemical formula. The larger the m and n, the larger the molecular weight and the higher the viscosity. Those skilled in the art can select the corresponding linear vinyl silicone oil according to the corresponding viscosity.
[0053] More preferably, in the linear vinyl silicone oil, the mass ratio of the low-viscosity material to the medium-viscosity material is 1:0.5 to 2.0, and more preferably 1:0.8 to 1.2.
[0054] More preferably, the mass ratio of the linear vinyl silicone oil to the overall material is 10-35%.
[0055] In a preferred embodiment, the branched vinyl silicone oil is a methyl vinyl polysiloxane with vinyl groups at both ends and in the middle of the molecular chain, and one molecule thereof contains at least 3 vinyl groups. Preferably, the chemical formula of the branched vinyl silicone oil is:
[0056] (CH2=CH)(CH3)2SiO[(CH3)2SiO] m [(CH2=CH)CH3SiO] n Si(CH3)2(CH2=CH).
[0057] More preferably, the mass ratio of the branched vinyl silicone oil to the overall material is 8-15%.
[0058] In a preferred embodiment, the hydrogen-containing silicone oil is a methyl polysiloxane containing Si-H groups in the middle of the molecular chain. Its hydrogen content is 0.6-1.5%, which belongs to high hydrogen-containing vinyl silicone oil. Preferably, the chemical formula of the hydrogen-containing silicone oil is:
[0059] (CH3)3SiO[RR'SiO] m [R'R"SiO] n Si(CH3)3, wherein R is H, R' is H or CH3, and R" is H or CH3.
[0060] In straight-chain vinyl silicone oil, the lower the material viscosity, the lower the molecular weight, and the higher the vinyl content. After the low-viscosity material is polymerized by silicon-hydrogen bonds in hydrogen-containing silicone oil, the polymer crosslinking density is high, but its molecular weight is small and the material toughness is insufficient; after the medium-viscosity material is polymerized by silicon-hydrogen bonds in hydrogen-containing silicone oil, the polymer crosslinking density is average, but its molecular weight is large and the material toughness is good. Through the synergistic effect of the two viscosity materials, and at the above addition ratio, the material has good toughness and will not affect its hardness.
[0061] In addition, the branched vinyl silicone oil and high hydrogen content vinyl silicone oil in the system can provide more cross-linking points for the material. The viscosity of the material is low before curing. After curing, the material has a high cross-linking density and a large molecular weight, providing a good foundation for the overall high hardness and low viscosity.
[0062] In a preferred embodiment, the vinyl MQ silicone resin has a general chemical formula:
[0063] (CH3)2(CH2=CH)SiO 1 / 2 ] a [(CH3)3SiO 1 / 2 ] b [SiO 4 / 2 ] c
[0064] Among them [(CH3)2(CH2=CH)SiO 1 / 2 ] a [(CH3)3SiO 1 / 2 ] b is the M group, [SiO 4 / 2 ] c It is a Q group.
[0065] Further preferably, the vinyl content in the vinyl MQ silicone resin is 1-3%; further preferably, the molar ratio of the M group to the Q group is 0.6-1.0. The vinyl MQ silicone resin is a spherical body with a double-layer structure. The core of the sphere is similar to an "inorganic structure", and the shell is an "organic group", which has both inorganic and organic characteristics. When the M / Q molar ratio is small, the silicone resin is in the form of particles and dispersed in the silicone rubber matrix in the form of loose aggregates, becoming the weakest part of the material with poor mechanical properties; with the increase of the M / Q molar ratio, the inorganic component in the silicone resin increases, and the reinforcement effect gradually improves, which is manifested as better mechanical properties; when the M / Q molar ratio increases to a certain extent, the organic component content is high, the compatibility of the silicone resin and silicone rubber becomes better, and it is evenly dispersed in the silicone rubber matrix, and the mechanical properties of the reinforced silicone rubber become worse. Therefore, the reinforcing effect of MQ silicone resin on silicone rubber is the result of the combined effect of the rigid O-Si-O core in MQ silicone resin and the compatibility of MQ silicone resin and silicone rubber. Under the above M / Q molar ratio, the reinforcing effect of MQ silicone resin on silicone rubber is better.
[0066] In a preferred embodiment, the nanofiller is hydrophobically treated nano-silicon dioxide or nano-alumina powder, and its average particle size is 5 to 100 nm, more preferably 10 to 30 nm;
[0067] The reinforcing filler is hydrophobically treated silica or alumina powder, and its average particle size is 5 to 100 μm, more preferably 10 to 50 μm;
[0068] The size and amount of filler particles are the most basic factors affecting the hardness and consistency of the material. The small size of nanoparticles is more conducive to uniform dispersion in the silicone rubber matrix, and is conducive to filling the small gap between the silicone rubber matrix and the coarse filler, thereby significantly increasing the hardness of the material, but it will also significantly increase the consistency of the product. Excessive addition will affect the use; the reinforcing particles have a larger particle size and have a smaller effect on the consistency of the product, and also have a certain reinforcing effect. The present invention can further improve the hardness of the product through the combined action of two fillers with different particle sizes, while not making the product too high in consistency.
[0069] In a preferred embodiment, the platinum catalyst is a Custer catalyst having a platinum content of 1% to 2%;
[0070] In a preferred embodiment, the plasticizer is liquid paraffin and / or white vaseline.
[0071] The high-hardness gun-mixed bite-recording silicone rubber of the embodiment of the present invention, the above raw materials are specifically divided into a matrix and a catalyst, calculated by weight percentage:
[0072] The matrix system includes: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogenated silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, and 0.5-5% plasticizer;
[0073] The catalyst system comprises: 10-50% straight-chain vinyl silicone oil, 5-25% branched-chain vinyl silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst and 0.5-5% plasticizer.
[0074] During preparation, the raw materials are weighed according to each component, and the matrix and catalyst system of the dental bite recording silicone rubber material are prepared separately by a kneading machine. Specifically, the materials of the matrix system are weighed, mixed by a kneading machine, and then vacuum degassed to prepare the matrix system; the materials of the catalyst system are weighed, mixed by a kneading machine, and then vacuum degassed to prepare the catalyst system; and the matrix system and the catalyst system are respectively filled into a two-component rubber cartridge. When in use, it is mixed by a mixing gun and then extruded. It can be understood by those skilled in the art that when extruding with a mixing gun, the matrix system and the catalyst system in the two-component rubber cartridge are extruded at the same time, and theoretically the volume ratio and mass ratio of the two are both 1:1.
[0075] In order to better illustrate and understand the product of the present invention, the following specific embodiments and comparative examples are provided, but the present invention is not limited to these embodiments:
[0076] The raw materials were weighed according to the components in the following examples and comparative examples, and the matrix and catalyst system of the dental silicone rubber bite recording material were prepared by a kneader. The kneader was mixed for 2 hours, and then vacuum degassed to prepare the matrix system and catalyst system, and the matrix and catalyst were filled into two-component rubber cartridges.
[0077] Examples 1 and 2
[0078]
[0079] Comparative Examples 1 and 2
[0080]
[0081]
[0082] The performance of the dental silicone rubber bite registration materials of the above examples and comparative examples was characterized.
[0083] The matrix component and the catalyst system component were filled into a 50 ml two-component cartridge and tested after mixing using a dental mixing gun.
[0084] The consistency, detail reproduction and linear size change of the samples were tested according to "YY 0493-2011 Dental Elastomer Impression Materials". The hardness of the samples was tested according to "GB / T2411-2008 Plastic Shore Hardness Test Method". The mixed material was pierced with an indenter with a weight of 400g and a needle diameter of 1mm. The time from the start of mixing to the time when the indenter could not be pressed in was the curing time.
[0085] The results are shown in the following table:
[0086]
[0087]
[0088] The results show that the consistency of Examples 1 to 2 and Comparative Example 1 is ≥35mm, and can be easily extruded and mixed evenly using a dental mixing gun. The detail reproduction, linear dimensional change, elastic recovery rate, and curing time all meet the clinical requirements of the product. The hardness of Examples 1 to 2 is ≥90, which meets the clinical requirements of the product. The hardness of Example 2 reaches 95, which is better than the hardness of general commercial products. The consistency of the product of Comparative Example 1 is appropriate, but due to the low content of branched vinyl silicone oil and nanofiller, the hardness is average; the hardness of the product of Comparative Example 2 is better, but there are more medium-viscosity materials in the linear vinyl silicone oil, which makes the overall consistency larger, and it takes more effort to mix with a gun, which is not suitable for clinical gun mixing.
[0089] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high hardness gun-mixed bite-recording silicone rubber, characterized in that: According to weight percentage, the raw materials include: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogen-containing silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst, 0.5-5% plasticizer.
2. The high hardness gun-mixed bite registration silicone rubber according to claim 1, characterized in that: The linear vinyl silicone oil is methyl vinyl polysiloxane or methyl phenyl vinyl polysiloxane with vinyl groups at both ends of the molecular chain, and one molecule thereof contains 2 vinyl groups; and / or, The branched vinyl silicone oil is a methyl vinyl polysiloxane having vinyl groups at both ends and in the middle of the molecular chain, and one molecule thereof contains at least 3 vinyl groups; and / or, The hydrogen-containing silicone oil is a methyl polysiloxane containing a Si-H group in the middle of the molecular chain.
3. The high hardness gun mixed bite registration silicone rubber according to claim 1, characterized in that: Including a matrix system and a catalyst system; in terms of weight percentage, The matrix system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogenated silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, and 0.5-5% plasticizer; The catalyst system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst and 0.5-5% plasticizer.
4. The high hardness gun-mixed bite registration silicone rubber according to any one of claims 1 to 3, characterized in that: The general chemical formula of the linear vinyl silicone oil is: (CH2=CH2)(CH3)2SiO[RR'SiO] m [R'R"SiO] n Si(CH3)2(CH2=CH2), wherein R is CH3 or C6H5, R' is CH3 or C6H5, and R" is CH3 or C6H5; and / or, The chemical formula of the branched vinyl silicone oil is: (CH2=CH)(CH3)2SiO[(CH3)2SiO] m [(CH2=CH)CH3SiO] n Si(CH3)2(CH2=CH); and / or, The general chemical formula of the hydrogen-containing silicone oil is: (CH3)3SiO[RR'SiO] m [R'R"SiO] n Si(CH3)3, wherein R is H, R' is H or CH3, and R" is H or CH3.
5. The high hardness gun-mixed bite registration silicone rubber according to any one of claims 1 to 3, characterized in that: The linear vinyl silicone oil comprises at least two materials with different viscosities; the viscosity range of the low viscosity material is 10-100 cst, and the viscosity range of the medium viscosity material is 200-1000 cst; preferably, the viscosity range of the low viscosity material is 20-50 cst, and the viscosity range of the medium viscosity material is 250-400 cst.
6. The high hardness gun mixed bite registration silicone rubber according to claim 5, characterized in that: In the linear vinyl silicone oil, the mass ratio of the low-viscosity material to the medium-viscosity material is 1:0.5-2.0, preferably 1:0.8-1.
2.
7. The high hardness gun mixed bite registration silicone rubber according to any one of claims 1 to 3 or 6, characterized in that: The general chemical formula of the vinyl MQ silicone resin is: <h2 style=";text-align:left;direction:ltr">(CH3)2(CH2=CH)SiO<h2 style=";text-align:left;direction:ltr"> 1 / 2 <h2 style=";text-align:left;direction:ltr"> ]<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> [(CH3)3SiO<h2 style=";text-align:left;direction:ltr"> 1 / 2 <h2 style=";text-align:left;direction:ltr"> ]<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> [SiO<h2 style=";text-align:left;direction:ltr"> 4 / 2 <h2 style=";text-align:left;direction:ltr"> ]<h2 style=";text-align:left;direction:ltr"> c Among them [(CH3)2(CH2=CH)SiO 1 / 2 ] a [(CH3)3SiO 1 / 2 ] b is the M group, [SiO 4 / 2 ] c is a Q group; Preferably, the molar ratio of the M group to the Q group is 0.6 to 1.
0.
8. The high hardness gun mixed bite registration silicone rubber according to any one of claims 1 to 3 or 6, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.6-1.5%; and / or, The vinyl MQ silicone resin has a vinyl content of 1 to 3%.
9. The high hardness gun mixed bite registration silicone rubber according to any one of claims 1 to 3 or 6, characterized in that: The nanofiller is hydrophobically treated nano-silicon dioxide and / or nano-alumina powder, preferably, the average particle size of the nanofiller is 5 to 100 nm; and / or, The reinforcing filler is hydrophobically treated silica and / or alumina powder, preferably, the average particle size of the reinforcing filler is 5 to 100 μm; and / or, The platinum catalyst is a Custer catalyst with a platinum content of 1% to 2%; and / or, The plasticizer is liquid paraffin and / or white vaseline.
10. The method for preparing the high hardness gun-mixed bite registration silicone rubber according to any one of claims 1 to 9, characterized in that: The steps include: Weigh the materials of the matrix system, mix them in a kneader, and then vacuum degas to prepare the matrix system; the matrix system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-8% hydrogenated silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, and 0.5-5% plasticizer; The materials of the catalyst system are weighed, mixed by a kneader, and then vacuum degassed to prepare a catalyst system; the catalyst system comprises: 10-50% linear vinyl silicone oil, 5-25% branched vinyl silicone oil, 2-10% vinyl MQ silicone resin, 1-9% nano filler, 20-55% reinforcing filler, 0.1%-2% platinum catalyst, and 0.5-5% plasticizer; The matrix system and the catalyst system are respectively filled into a two-component rubber cartridge.