Multi-angle color-changing film for road sign and preparation process of multi-angle color-changing film

Through the multi-angle color change film process, multi-angle color change paint is prepared using materials such as polyurethane acrylate and applied to road signs, solving the problem that fixed color marks are difficult to identify in high-speed environments, improving weather resistance and wear resistance, and enhancing security.

CN118931305AActive Publication Date: 2024-11-12NALINKO NEW MATERIALS (NANTONG) CO LTD

Patent Information

Application Number
CN202411231455.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The fixed color markings of existing road signs are difficult to quickly and accurately identify under high-speed driving or complex traffic environments, which poses safety risks, and traditional methods have failed to fundamentally change this limitation.

Method used

Using a multi-angle color change film process, acrylic resin is prepared by reaction of polyurethane acrylate, UV-proof agent, styrene, ethyl acrylate and other materials, and metal pigments and drying agent are added to form a multi-angle color change paint and coated on road signs. The surface is displayed using angle changes to display different colors to improve recognition.

Benefits of technology

It improves the weather resistance, wear resistance and pollution resistance of road signs, enhances the driver's ability to identify lanes during rapid driving, and reduces traffic safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of multi-angle color-changing films, and particularly discloses a multi-angle color-changing film for a road sign and a preparation process of the multi-angle color-changing film. The preparation process of the multi-angle color-changing film comprises the following steps: S1, dissolving hydroxyethyl methylacrylate in a solvent, adding diisocyanate, 4, 4 '-dihydroxybenzophenone and 2, 2, 6, 6-tetramethyl piperidylamine, stirring to react until the content of isocyanato is not reduced any more, and removing the solvent to obtain an anti-ultraviolet agent; s2, taking urethane acrylate, an anti-ultraviolet agent, styrene, ethyl acrylate and methyl methacrylate, uniformly mixing, adding benzoyl peroxide, and carrying out reaction polymerization to obtain acrylic resin; s3, adding the metal pigment into the n-butyl acetate, and uniformly stirring; adding a metal pigment orientation agent and acrylic resin, uniformly dispersing, and adding a drier for dispersing to obtain a multi-angle color-changing coating; and coating the surface of the road sign with the multi-angle color-changing coating, and drying to obtain the multi-angle color-changing film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of multi-angle color-changing films, and in particular discloses a multi-angle color-changing film for a road sign and a preparation process thereof. Background Art

[0002] At present, road signs generally use fixed-color logos to indicate different lanes. However, this method may be difficult for drivers to quickly and accurately identify their own lanes when driving at high speeds or in complex traffic environments, which poses certain safety risks. The traditional solution is to set more eye-catching logos on road signs or increase the number of logos to improve recognition. However, these methods do not fundamentally change the limitations of fixed-color logos.

[0003] Coating a multi-angle color-changing film on a road sign can display different colors according to the viewing angle, so that drivers can quickly distinguish the lanes they are in during fast driving, reducing traffic safety hazards. Therefore, it is of great significance to study a multi-angle color-changing film for road signs with good weather resistance, good wear resistance, and good antifouling properties and its preparation process. Summary of the invention

[0004] The object of the present invention is to provide a multi-angle color-changing film for road signs and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a preparation process of a multi-angle color-changing film for a road sign, characterized in that it comprises the following steps: S1: dissolving hydroxyethyl methacrylate in a solvent, adding diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring and reacting until the isocyanate content no longer decreases, and removing the solvent to obtain a UV protector; S2: Take polyurethane acrylate, UV protection agent, styrene, ethyl acrylate, and methyl methacrylate, mix them evenly, add benzoyl peroxide, react and polymerize to obtain acrylic resin; S3: Add metal pigment to butyl acetate and stir evenly; add metal pigment directing agent and acrylic resin, disperse evenly, and then add drying agent to disperse, so as to obtain multi-angle color-changing paint; apply the multi-angle color-changing paint to the surface of the road sign, dry it, and obtain a multi-angle color-changing film.

[0006] More optimally, in the anti-ultraviolet agent, the molar ratio of hydroxyethyl methacrylate, diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1: (2-2.2): (0.8-1): (0.8-1); the diisocyanate is isophorone diisocyanate; the solvent is acetone; and the amount of acetone added is 12 times that of hydroxyethyl methacrylate; The acrylic resin comprises the following raw materials, calculated by weight: 30-35 parts of polyurethane acrylate, 10-15 parts of UV protection agent, 20-25 parts of styrene, 30-35 parts of ethyl acrylate, 5-8 parts of methyl methacrylate, and 1.5-2 parts of benzoyl peroxide; The multi-angle color-changing coating includes the following raw materials, calculated by mass: 5 to 8 parts of metallic pigment, 15 to 20 parts of butyl acetate, 8 to 12 parts of metallic pigment directing agent, 70 to 80 parts of acrylic resin, and 0.01 to 0.02 parts of drying agent; the drying agent is dibutyltin dilaurate; and the metallic pigment directing agent is cellulose acetate butyrate.

[0007] More optimally, the preparation of the polyurethane acrylate includes the following steps: taking polytetramethylene glycol, 5-henedecylresorcinol, acetone, and water, stirring evenly, heating, adding diisocyanate and dibutyltin dilaurate, stirring and reacting to obtain a prepolymer; adding trimethylolpropane, reacting at 60-65°C for 1-2h, adding modified sodium alginate and hydroxyethyl methacrylate, continuing to stir and react until the isocyanate content no longer decreases, and removing the solvent by rotary evaporation to obtain polyurethane acrylate.

[0008] More optimally, the polyurethane acrylate includes the following raw materials, calculated by mass: 10 to 15 parts of polytetramethylene glycol, 5 to 8 parts of 5-henedecylresorcinol, 20 to 25 parts of acetone, 5 to 8 parts of water, 10 to 15 parts of diisocyanate (isophorone diisocyanate), 0.5 to 0.8 parts of dibutyltin dilaurate, 5 to 6 parts of trimethylolpropane, 2 to 3 parts of modified sodium alginate, and 6 to 10 parts of hydroxyethyl methacrylate.

[0009] More optimally, the preparation of the modified sodium alginate includes the following steps: taking sodium alginate, adding a mixed solvent, adding 2,4-difluorophenyl isocyanate, mixing evenly, stirring the reaction until the isocyanate content no longer decreases, and removing the mixed solvent to obtain modified sodium alginate.

[0010] More optimally, the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:(1-1.2); the mixed solvent is water and acetone in a volume ratio of 3:1, and the added amount is 10 times the mass of sodium alginate.

[0011] More optimally, the coating thickness of the multi-angle color-changing coating is 20-30 μm.

[0012] More optimally, the specific drying process is: baking at 75-80°C for 110-120 minutes.

[0013] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the acrylic resin used for preparing the multi-angle color-changing coating of the present invention is obtained by polymerizing a certain amount of polyurethane acrylate, UV protection agent, styrene, ethyl acrylate and methyl methacrylate; Among them, polyurethane acrylate has good wear resistance. The raw materials also include 5-henedecylresorcinol, which is hydrophobic and can effectively improve the anti-corrosion and waterproof and anti-fouling properties of the coating; trimethylolpropane is added to make it have a hyperbranched structure, improve mechanical properties and have good fluidity and film-forming properties. The end is also grafted with sodium alginate modified with 2,4-difluorophenyl isocyanate. Due to the presence of fluorine and benzene, the affinity and repellency of the modified sodium alginate are adjusted, and it has emulsification ability and can help disperse metal pigments; therefore, there is no need to add additional leveling agents, dispersants and other additives; The anti-ultraviolet agent prepared by the present invention is obtained by compounding hydroxyethyl methacrylate, diisocyanate, 4,4'-dihydroxybenzophenone and 2,2,6,6-tetramethylpiperidinamine, wherein the anti-ultraviolet agent contains double bonds and can participate in polymerization reaction, thereby improving the problems of poor dispersibility and compatibility when the anti-ultraviolet agent is directly added, and also improving the problem of precipitation resulting in performance degradation when small molecule additives are directly added. DETAILED DESCRIPTION

[0014] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0015] The following parts are by mass unless otherwise specified; Example 1: S1: Take sodium alginate, add a mixed solvent, add 2,4-difluorophenyl isocyanate, mix well, stir and react at 55°C until the isocyanate content no longer decreases, remove the mixed solvent, and obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1; S2: Add 12 parts of polytetrahydrofuran diol, 6 parts of 5-henedecylresorcinol, 25 parts of acetone and 5 parts of water to a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 12 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 2 hours to obtain a prepolymer; add 5 parts of trimethylolpropane, react at 65°C for 2 hours, add 3 parts of modified sodium alginate and 8 parts of hydroxyethyl methacrylate, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain polyurethane acrylate; S3: dissolving hydroxyethyl methacrylate in acetone, adding isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring evenly, reacting at 55° C. until the isocyanate content no longer decreases, removing the solvent, and obtaining an anti-ultraviolet agent; the molar ratio of hydroxyethyl methacrylate, isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:2.2:0.8:1; S4: Take 32 parts of polyurethane acrylate, 12 parts of UV protection agent, 25 parts of styrene, 30 parts of ethyl acrylate, and 6 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S5: Take 6 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 10 parts of cellulose acetate butyrate and 75 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0016] Example 2: S1: Take sodium alginate, add a mixed solvent, add 2,4-difluorophenyl isocyanate, mix well, stir and react at 55°C until the isocyanate content no longer decreases, remove the mixed solvent, and obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1.2; S2: Add 15 parts of polytetrahydrofuran diol, 8 parts of 5-henedecylresorcinol, 25 parts of acetone and 5 parts of water into a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 15 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 2 hours to obtain a prepolymer; add 6 parts of trimethylolpropane, react at 65°C for 2 hours, add 3 parts of modified sodium alginate and 10 parts of hydroxyethyl methacrylate, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain polyurethane acrylate; S3: dissolving hydroxyethyl methacrylate in acetone, adding isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring evenly, reacting at 55° C. until the isocyanate content no longer decreases, removing the solvent, and obtaining an anti-ultraviolet agent; the molar ratio of hydroxyethyl methacrylate, isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:2.2:1:0.8; S4: Take 35 parts of polyurethane acrylate, 10 parts of UV protection agent, 20 parts of styrene, 35 parts of ethyl acrylate, and 5 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S5: Take 8 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 12 parts of cellulose acetate butyrate and 80 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, and disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0017] Example 3: S1: Take sodium alginate, add a mixed solvent, add 2,4-difluorophenyl isocyanate, mix well, stir and react at 55°C until the isocyanate content no longer decreases, remove the mixed solvent, and obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1; S2: Add 10 parts of polytetrahydrofuran diol, 5 parts of 5-henedecylresorcinol, 25 parts of acetone and 5 parts of water into a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 10 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 2 hours to obtain a prepolymer; add 6 parts of trimethylolpropane, react at 65°C for 2 hours, add 2 parts of modified sodium alginate and 6 parts of hydroxyethyl methacrylate, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain polyurethane acrylate; S3: dissolving hydroxyethyl methacrylate in acetone, adding isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring evenly, stirring and reacting at 55° C. until the isocyanate content no longer decreases, removing the solvent, and obtaining an anti-ultraviolet agent; the molar ratio of hydroxyethyl methacrylate, isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:2:0.8:0.8; S4: Take 30 parts of polyurethane acrylate, 10 parts of UV protection agent, 20 parts of styrene, 30 parts of ethyl acrylate, and 5 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, react at 80°C for 6 hours, and obtain acrylic resin; S5: Take 5 parts of metallic pigment, add 15 parts of butyl acetate, and stir evenly; add 8 parts of cellulose acetate butyrate and 70 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, and disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0018] Comparative Example 1 (modified sodium alginate is not introduced, and the remaining steps are consistent with those of Example 1): S1: 12 parts of polytetrahydrofuran diol, 6 parts of 5-henedecylresorcinol, 25 parts of acetone, and 5 parts of water are added to a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser, and a nitrogen conduit, and stirred evenly. After heating to 70° C., 12 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate are added, and stirred for reaction for 2 hours to obtain a prepolymer; 5 parts of trimethylolpropane are added, and the mixture is reacted at 65° C. for 2 hours, and 11 parts of hydroxyethyl methacrylate are added, and the reaction is continued by stirring until the content of isocyanate no longer decreases, the reaction is stopped, and the solvent is removed by rotary evaporation to obtain polyurethane acrylate; S2: dissolving hydroxyethyl methacrylate in acetone, adding isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring evenly, stirring and reacting at 55° C. until the isocyanate content no longer decreases, removing the solvent, and obtaining an anti-ultraviolet agent; the molar ratio of hydroxyethyl methacrylate, isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:2.2:0.8:1; S3: Take 32 parts of polyurethane acrylate, 12 parts of UV protection agent, 25 parts of styrene, 30 parts of ethyl acrylate, and 6 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S4: Take 6 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 10 parts of cellulose acetate butyrate and 75 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, and disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0019] Comparative Example 2 (trimethylolpropane is not introduced, and the remaining steps are consistent with those of Example 1): S1: sodium alginate is taken, a mixed solvent is added, 2,4-difluorophenyl isocyanate is added, the mixture is uniformly mixed, and the mixture is stirred at 55° C. to react until the isocyanate content no longer decreases, and the mixed solvent is removed to obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1; S2: Add 12 parts of polytetrahydrofuran diol, 6 parts of 5-henedecylresorcinol, 25 parts of acetone and 5 parts of water to a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 12 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 4 hours, add 3 parts of modified sodium alginate and 8 parts of hydroxyethyl methacrylate, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain polyurethane acrylate; S3: dissolving hydroxyethyl methacrylate in acetone, adding isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring evenly, reacting at 55° C. until the isocyanate content no longer decreases, removing the solvent, and obtaining an anti-ultraviolet agent; the molar ratio of hydroxyethyl methacrylate, isophorone diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:2.2:0.8:1; S4: Take 32 parts of polyurethane acrylate, 12 parts of UV protection agent, 25 parts of styrene, 30 parts of ethyl acrylate, and 6 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S5: Take 6 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 10 parts of cellulose acetate butyrate and 75 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0020] Comparative Example 3 (4,4'-dihydroxybenzophenone and 2,2,6,6-tetramethylpiperidinamine are directly added as UV protection agents, and the remaining steps are consistent with those of Example 1): S1: sodium alginate is taken, a mixed solvent is added, 2,4-difluorophenyl isocyanate is added, the mixture is mixed evenly, and the mixture is stirred at 55°C to react until the isocyanate content no longer decreases, and the mixed solvent is removed to obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1; S2: Add 12 parts of polytetrahydrofuran diol, 6 parts of 5-henedecylresorcinol, 25 parts of acetone and 5 parts of water to a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 12 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 2 hours to obtain a prepolymer; add 5 parts of trimethylolpropane, react at 65°C for 2 hours, add 3 parts of modified sodium alginate and 8 parts of hydroxyethyl methacrylate, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain polyurethane acrylate; S3: taking 4,4'-dihydroxybenzophenone and 2,2,6,6-tetramethylpiperidinamine in a molar ratio of 0.8:1, and mixing them to obtain a UV protection agent; S4: Take 32 parts of polyurethane acrylate, 12 parts of UV protection agent, 25 parts of styrene, 30 parts of ethyl acrylate, and 6 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S5: Take 6 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 10 parts of cellulose acetate butyrate and 75 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0021] Comparative Example 4 (modified polyurethane acrylate is used instead of polyurethane acrylate and anti-ultraviolet agent, and the other method steps are consistent with Example 1): S1: sodium alginate is taken, a mixed solvent is added, 2,4-difluorophenyl isocyanate is added, mixed evenly, stirred at 55° C. to react until the isocyanate content no longer decreases, and the mixed solvent is removed to obtain modified sodium alginate; the molar ratio of sodium alginate to 2,4-difluorophenyl isocyanate is 1:1; S2: Add 10 parts of polytetrahydrofuran diol, 5 parts of 5-henedecylresorcinol, 3 parts of 4,4'-dihydroxybenzophenone, 25 parts of acetone and 5 parts of water to a three-necked flask equipped with a polytetrafluoroethylene stirring rod, a condenser and a nitrogen conduit, stir evenly, heat to 70°C, add 12 parts of isophorone diisocyanate and 0.6 parts of dibutyltin dilaurate, stir and react for 2 hours to obtain a prepolymer; add 5 parts of trimethylolpropane, react at 65°C for 2 hours, add 3 parts of modified sodium alginate, 5 parts of hydroxyethyl methacrylate and 3 parts of 2,2,6,6-tetramethylpiperidinamine, continue to stir and react until the isocyanate content no longer decreases, stop the reaction, and remove the solvent by rotary evaporation to obtain a modified polyurethane acrylate; S3: Take 44 parts of modified polyurethane acrylate, 25 parts of styrene, 30 parts of ethyl acrylate, and 6 parts of methyl methacrylate, mix them evenly, add 1.5 parts of benzoyl peroxide, and react at 80°C for 6 hours to obtain acrylic resin; S4: Take 6 parts of metallic pigment, add 20 parts of butyl acetate, and stir evenly; add 10 parts of cellulose acetate butyrate and 75 parts of acrylic resin, disperse for 20 minutes at a speed of 2000r / min, then add 0.01 parts of drier dibutyltin dilaurate, and disperse for 20 minutes to obtain a multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign with a coating thickness of 25μm, and bake at 80℃ for 120 minutes to obtain a multi-angle color-changing film.

[0022] In the above examples, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: acetone (CAS: 67-64-1); 2,4-difluorophenyl isocyanate (S48727, Shanghai Yuanye); sodium alginate (S11053, Shanghai Yuanye); polytetrahydrofuran diol (PTMG-1000, Shandong Suihua Biotechnology Co., Ltd.); 5-henedecylresorcinol (B32973, Shanghai Yuanye); isophorone diisocyanate (CAS: 4098-71-9); dilaurate diisocyanate (CAS: 4098-71-9); Butyltin (CAS: 77-58-7); Trimethylolpropane (CAS: 77-99-6); Hydroxyethyl methacrylate (CAS: 868-77-9); 4,4'-Dihydroxybenzophenone (CAS: 611-99-4); 2,2,6,6-Tetramethylpiperidinamine (CAS: 36768-62-4); Styrene (CAS: 100-42-5); Ethyl acrylate (CAS: 140-88-5); Methyl methacrylate (CAS: 80-62-6); Benzoyl peroxide (CAS: 94-36-0); Metallic pigments (Merck colorstream series, Autumn Mystery); Butyl acetate (CAS: 123-86-4); Cellulose acetate butyrate (CAS: 9004-36-8).

[0023] Experiment: The multi-angle color-changing coatings prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were applied to a mold with a coating thickness of 25 μm to obtain a sample film; (1) with reference to GBT14522-2008, artificial accelerated aging for 1000 h was performed to test the gloss retention rate; (2) with reference to GB / T1768-2006, abrasion resistance was tested; (3) a contact angle meter was used to measure the water contact angle; specific data are shown in the table below;

[0024] Conclusion: Comparative Example 1 did not introduce modified sodium alginate, and the performance was reduced; Comparative Example 2 did not introduce trimethylolpropane, the branched structure of polyurethane acrylate was reduced, and the performance was not as good as the embodiment; Comparative Example 3 directly added 4,4'-dihydroxybenzophenone and 2,2,6,6-tetramethylpiperidinamine as anti-ultraviolet agents, and due to the small molecular weight, there were problems of uneven dispersion or migration, resulting in decreased performance; Comparative Example 4 used modified polyurethane acrylate instead of polyurethane acrylate and anti-ultraviolet agent, and due to problems such as grafting rate and steric hindrance, the performance was not as good as the embodiment; In summary, the multi-angle color-changing film for road signs prepared by the present invention has good weather resistance, good wear resistance, and good hydrophobic and anti-fouling properties.

[0025] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A process for preparing a multi-angle color-changing film for a road sign, characterized in that: The following steps are involved: S1: dissolving hydroxyethyl methacrylate in a solvent, adding diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine, stirring and reacting until the isocyanate content no longer decreases, and removing the solvent to obtain a UV protector; S2: Take polyurethane acrylate, UV protection agent, styrene, ethyl acrylate, and methyl methacrylate, mix them evenly, add benzoyl peroxide, react and polymerize to obtain acrylic resin; S3: Add metal pigment to butyl acetate and stir evenly; add metal pigment directing agent and acrylic resin, disperse evenly, then add drying agent, disperse evenly to obtain multi-angle color-changing paint; apply the multi-angle color-changing paint on the surface of the road sign, dry it, and obtain a multi-angle color-changing film.

2. The process for preparing a multi-angle color-changing film for a road sign according to claim 1, characterized in that: In the anti-ultraviolet agent, the molar ratio of hydroxyethyl methacrylate, diisocyanate, 4,4'-dihydroxybenzophenone, and 2,2,6,6-tetramethylpiperidinamine is 1:(2-2.2):(0.8-1):(0.8-1); The acrylic resin comprises the following raw materials, calculated by weight: 30-35 parts of polyurethane acrylate, 10-15 parts of UV protection agent, 20-25 parts of styrene, 30-35 parts of ethyl acrylate, 5-8 parts of methyl methacrylate, and 1.5-2 parts of benzoyl peroxide; The multi-angle color-changing paint includes the following raw materials, calculated by weight: 5 to 8 parts of metallic pigment, 15 to 20 parts of butyl acetate, 8 to 12 parts of metallic pigment directing agent, 70 to 80 parts of acrylic resin, and 0.01 to 0.02 parts of drying agent.

3. The process for preparing a multi-angle color-changing film for a road sign according to claim 1, characterized in that: The preparation of the polyurethane acrylate comprises the following steps: Take polytetrahydrofuran diol, 5-henedecylresorcinol, acetone and water, stir evenly, heat up, add diisocyanate and dibutyltin dilaurate, stir and react to obtain a prepolymer; add trimethylolpropane, react at 60-65°C for 1-2h, add modified sodium alginate and hydroxyethyl methacrylate, continue stirring and reacting until the isocyanate content no longer decreases, and remove the solvent by rotary evaporation to obtain polyurethane acrylate.

4. The process for preparing a multi-angle color-changing film for a road sign according to claim 3, characterized in that: The polyurethane acrylate comprises the following raw materials, calculated by weight: 10-15 parts of polytetramethylene glycol, 5-8 parts of 5-henedecylresorcinol, 20-25 parts of acetone, 5-8 parts of water, 10-15 parts of diisocyanate, 0.5-0.8 parts of dibutyltin dilaurate, 5-6 parts of trimethylolpropane, 2-3 parts of modified sodium alginate, and 6-10 parts of hydroxyethyl methacrylate.

5. The process for preparing a multi-angle color-changing film for a road sign according to claim 3, characterized in that: The preparation of the modified sodium alginate comprises the following steps: Take sodium alginate, add a mixed solvent, add 2,4-difluorophenyl isocyanate, mix evenly, stir to react until the isocyanate content no longer decreases, remove the mixed solvent, and obtain modified sodium alginate.

6. The process for preparing a multi-angle color-changing film for a road sign according to claim 5, characterized in that: The molar ratio of the sodium alginate to 2,4-difluorophenyl isocyanate is 1:(1-1.2).

7. The process for preparing a multi-angle color-changing film for a road sign according to claim 1, characterized in that: The coating thickness of the multi-angle color-changing coating is 20-30 μm.

8. The process for preparing a multi-angle color-changing film for a road sign according to claim 1, characterized in that: The specific drying process is: baking at 75-80°C for 110-120 minutes.

9. A multi-angle color-changing film obtained according to the preparation process of a multi-angle color-changing film for road signs according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of heulandite nano-powder modified aqueous polyurethane anti-wear coating

    CN107163827A

  • Multi-angle color changing paint for automobile badges and preparation method thereof

    CN109749558A

  • Coating composition for ultraviolet curing and accessory ornaments using the same

    KR100731209B1

  • Photo-curable urethane acrylate containing UV-absorberfunctional groups and process for preparing thereof,and its photo-curable resin composition

    KR1020030080712A

  • Methacrylate resins for producing road markings

    US20090253845A1

Cited By

  • Waterborne polyurethane / acrylate hybrid resin dispersion liquid as well as preparation method and application thereof

    CN120775116A

  • A waterborne polyurethane / acrylate hybrid resin dispersion, its preparation method and application

    CN120775116B