Preparation method of outer-layer heat dissipation coating for electric appliance cabinet
By using acidification and ultrasonic dispersed multi-wall carbon nanotubes and metal nanoparticles modification, combined with the bridging of expanded graphite, an efficient outer heat dissipation coating of electrical cabinets was prepared, which solved the problem of low heat dissipation efficiency of electronic equipment and significantly improved the Thermal conductivity and adhesion extend the service life of the equipment.
Patent Information
- Application Number
- CN202411028138.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
Existing methods of cooling of electronic equipment such as air cooling and liquid cooling have limitations. The limit of cooling of air cooling is inconsistent with the trend of miniaturization and miniaturization of electronic devices. The liquid cooling system is complex, heavy and expensive, resulting in low heat dissipation efficiency of electronic equipment, affecting Reliability and service life.
Multi-walled carbon nanotubes and modified multi-walled carbon nanotubes are used as composite fillers, and an efficient thermal conductivity network is formed through acidification treatment, ultrasonic dispersion and metal nanoparticles modification. Combined with the bridging of expanded graphite, an efficient outer layer of electrical cabinet is prepared. Heat dissipation coating.
It significantly improves the thermal conductivity and adhesion of the heat dissipation coating, solves the problem of excellent axial thermal conductivity but poor radial heat exchange performance of multi-wall carbon nanotubes, enhances the heat dissipation ability of electronic equipment, extends service life and reduces faults Rate.
Smart Images

Figure BDA0004969155860000101 
Figure BDA0004969155860000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer coating materials, in particular to a method for preparing an outer heat dissipation coating for an electrical cabinet. Background Art
[0002] With the rapid development of electronic components, the system integration is constantly improving, resulting in high heat density becoming a significant development trend. This trend has significantly increased the frequency of electronic equipment failures caused by poor heat dissipation. According to surveys, more than 40% of electronic product reliability failures are caused by temperature problems. For every 10°C increase in the temperature of electronic parts, their service life will be reduced by half. Therefore, effectively solving the heat dissipation problem of electronic components has become a key technology that needs to be urgently solved in the development of the information industry.
[0003] At present, the commonly used heat dissipation methods mainly include air cooling and liquid cooling. The heat dissipation limit of the air cooling system is 40W / cm 2 To further increase the heat dissipation, the heat dissipation space must be expanded, but this is contrary to the current development trend of miniaturization, miniaturization and precision of electronic devices. In contrast, the heat dissipation capacity of the liquid cooling system is 1 to 2 orders of magnitude higher than that of the air cooling system, but its cooling system is relatively complex, with large volume and weight, and high equipment and maintenance costs.
[0004] In view of the above problems, heat dissipation coatings, as a special coating that improves the heat dissipation efficiency of the surface of objects and reduces the system temperature, have become an important direction for solving the heat dissipation problem of electronic products due to its simple and economical preparation method. Heat dissipation coatings effectively enhance heat dissipation and reduce the operating temperature of electronic components by forming a high thermal conductivity coating on the surface of electronic equipment, thereby extending their service life and improving their reliability.
[0005] In particular, the application of heat dissipation coatings on the outer layer of electrical cabinets can not only effectively solve the heat dissipation problem of internal electronic components, but also reduce equipment failures caused by excessive temperature. The preparation and application of heat dissipation coatings on the outer layer of electrical cabinets will provide important guarantees for the reliable operation of electronic equipment, and have broad application prospects and significant economic benefits.
[0006] Therefore, it is of great significance to invent a heat dissipation coating that is efficient, economical and suitable for the outer layer of an electrical cabinet. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing a heat dissipation coating for the outer layer of an electrical cabinet, so as to solve the problems raised in the above-mentioned background technology.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0009] A method for preparing a heat dissipation coating for an outer layer of an electrical cabinet comprises the following steps:
[0010] S1: Add xylene and butyl acetate to solvent oil, stir evenly to obtain a mixed solvent; add filler and nano alloy powder to the mixed solvent, stir evenly, add nano dispersant and defoamer, stir evenly, ultrasonically disperse for 1-2h, add modified polyurethane and polyurethane modified epoxy resin, stir evenly to obtain component A;
[0011] S2: adding the curing agent into a mixed solvent consisting of xylene, butyl acetate and solvent oil, stirring evenly to obtain component B;
[0012] S3: Mix component A and component B evenly according to a certain proportion to obtain a heat dissipation coating.
[0013] Furthermore, the proportions of the components in component A, by mass, are 30-50 parts of modified polyurethane, 20-40 parts of polyurethane modified epoxy resin, 5-10 parts of filler, 1-5 parts of nano-dispersant, 0.2-0.5 parts of defoaming agent, 10-20 parts of nano-alloy powder, 30-50 parts of solvent oil, 30-50 parts of xylene, and 30-50 parts of butyl acetate.
[0014] Furthermore, the proportions of the components in the B component, by mass, are 1-10 parts of curing agent, 30-50 parts of xylene, 30-50 parts of butyl acetate, and 30-50 parts of solvent oil.
[0015] Furthermore, the modified polyurethane is a hydroxyl-terminated polyurethane synthesized from aliphatic isocyanate and diol; the diol includes any one or more of ethylene glycol, butanediol, diethylene glycol, and hexanediol.
[0016] Furthermore, the aliphatic isocyanate includes trimethyl hexamethylene diisocyanate; and the preparation method of the modified polyurethane includes the following steps:
[0017] Add diol into a reaction vessel, treat at 90-100°C, -0.08MPa for 2-3h, cool to 50-60°C, add aliphatic isocyanate according to the molar ratio of -NCO to -OH (4-5):1, heat to 70-80°C and react for 3-4h to obtain modified polyurethane.
[0018] Furthermore, the aliphatic isocyanate includes trimethyl hexamethylene diisocyanate (a mixture of 2,2,4- and 2,4,4-); and the diol includes any one or more of ethylene glycol, butanediol, diethylene glycol, and hexanediol.
[0019] Furthermore, the polyurethane modified epoxy resin has an epoxy equivalent of 500-700.
[0020] Furthermore, the preparation method of the polyurethane modified epoxy resin comprises the following steps:
[0021] The isocyanate monomer and any one of the polyether diols or polyester diols are mixed according to the molar ratio of -NCO to -OH (3-
[0022] 4):1 mixed and heated to 60-90°C for reaction for 2-4h to synthesize a prepolymer containing an isocyanate group end-capping, and the polyol containing an epoxy group and the prepolymer are mixed and reacted for 60-90s according to the molar ratio of -NCO to -OH (1.05-1.1):1 to obtain a polyurethane modified epoxy resin;
[0023] Further, the isocyanate monomer includes any one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, and hexamethylene diisocyanate;
[0024] Further, the polyether diol includes polyether N-210; the polyester diol includes polybutylene adipate diol, 1,4-butylene adipate diol;
[0025] Furthermore, the epoxy group-containing polyol includes aliphatic polyol glycidyl ether; the aliphatic polyol glycidyl ether includes any one or more of polyethylene glycol diglycidyl ether and polyglycerol diglycidyl ether.
[0026] Furthermore, the filler includes any one or two of multi-walled carbon nanotubes and modified multi-walled carbon nanotubes, the multi-walled carbon nanotubes in the multi-walled carbon nanotubes and the modified multi-walled carbon nanotubes have a diameter of 10-100nm and a length of 2-3μm; the nano alloy powder includes any one or more of nano silicon aluminum alloy powder, nano silicon aluminum oxygen carbon alloy powder, and nano aluminum carbon alloy powder; the curing agent includes any one or two of imidazoles and dicyandiamide.
[0027] Furthermore, the mass ratio of component A to component B is 100:(5-20).
[0028] Furthermore, the filler is composed of multi-walled carbon nanotubes and modified multi-walled carbon nanotubes in a mass ratio of (4-6):(4-6).
[0029] Furthermore, the method for preparing the modified multi-walled carbon nanotubes comprises the following steps:
[0030] Step (1): adding multi-walled carbon nanotubes to a mixed solution of concentrated nitric acid and concentrated hydrochloric acid, ultrasonically dispersing for 30-45 minutes, heating to 75-80° C. and stirring for 24 hours, diluting the mixture in deionized water in a fume hood, precipitating, removing the supernatant, repeating the operation until there is no supernatant, centrifuging the precipitated mixed solution, removing the supernatant, washing the precipitate to a pH of 7-7.2, and vacuum drying at 60-80° C. to obtain carboxylated multi-walled carbon nanotubes;
[0031] Step (2): dissolving polyvinyl alcohol in N,N-dimethylformamide, adding carboxylated multi-walled carbon nanotubes, heating to 80-85°C, ultrasonically treating for 1-1.5h, filtering using a filter membrane with a pore size of 0.4-0.45mm to obtain a filtrate; preheating the filtrate to 80-85°C, adding an aqueous solution of aluminum nitrate, keeping warm and stirring for 2-2.5h, adding ammonia water to a pH of 9-10, filtering, washing, vacuum drying at 80-85°C, grinding, and calcining at 495-505°C for 2-2.5h to obtain hybrid multi-walled carbon nanotubes;
[0032] Step (3): adding silver nitrate crystals and benzyl mercaptan to ethanol, stirring evenly, adding a mixed solution consisting of carboxylated multi-walled carbon nanotubes, N,N-dimethylformamide, 4,4'-diaminodiphenyl ether, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine, heating to 60-65° C. for reaction for 4-5 days, centrifuging, removing the supernatant, washing the precipitate to a pH of 7-7.2, and vacuum drying at 60-65° C. to obtain composite multi-walled carbon nanotubes;
[0033] Step (4): adding hybrid multi-walled carbon nanotubes and composite multi-walled carbon nanotubes to a sodium dodecylbenzene sulfonate solution, ultrasonically treating for 30-45 minutes, filtering, washing, vacuum drying at 80-85° C., and grinding to obtain negatively charged multi-walled carbon nanotubes; adding expanded graphite to a hexadecyltrimethylammonium bromide solution, ultrasonically treating for 30-45 minutes, filtering, washing, vacuum drying at 80-85° C., and grinding to obtain positively charged expanded graphite; adding negatively charged multi-walled carbon nanotubes and positively charged expanded graphite to deionized water, ultrasonically treating for 30-45 minutes, filtering, vacuum drying, and grinding to obtain modified multi-walled carbon nanotubes.
[0034] Furthermore, in step (1), the volume ratio of concentrated nitric acid to concentrated hydrochloric acid is 1:3;
[0035] Furthermore, in the step (2), the mass fraction of polyvinyl alcohol dissolved in N,N-dimethylformamide is 2-3%, and the mass fraction of aluminum nitrate aqueous solution is 10-12%;
[0036] Furthermore, in the step (3), the molar ratio of silver nitrate crystals to benzyl mercaptan is 100:(6.7-8.4), the mass ratio of carboxylated multi-walled carbon nanotubes to 4,4'-diaminodiphenyl ether to dicyclohexylcarbodiimide to 4-dimethylaminopyridine is (1-2):(20-30):(10-18):(6-10), and the mass ratio of silver nitrate crystals to carboxylated multi-walled carbon nanotubes is 1:1;
[0037] Furthermore, in step (4), the mass ratio of hybrid multi-walled carbon nanotubes: composite multi-walled carbon nanotubes: positively charged expanded graphite is 1:1:1, the concentration of the sodium dodecylbenzenesulfonate solution is 1-2 g / L, and the concentration of the hexadecyltrimethylammonium bromide solution is 9-10 g / L.
[0038] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0039] The present invention selects multi-walled carbon nanotubes and modified multi-walled carbon nanotubes as composite fillers to solve the problem that the multi-walled carbon nanotubes have excellent axial heat conduction performance and poor radial heat exchange performance. The present invention first acidifies the multi-walled carbon nanotubes so that the surface carries a large number of carboxyl functional groups, and then ultrasonically treats them in a polyvinyl alcohol solution (on the one hand, polyvinyl alcohol is grafted on the surface of the carboxylated multi-walled carbon nanotubes, on the other hand, the carboxylated carbon nanotube line can be cut into shorter pipes by strong ultrasonic treatment, and the dispersion performance and grafting rate in polyvinyl alcohol are improved. At the same time, the multi-walled carbon nanotubes with shorter lengths can improve the density in the polyurethane matrix, and the multi-walled carbon nanotubes are fully contacted to form a perfect heat conduction network, greatly improving the thermal conductivity, avoiding the introduction of longer multi-walled carbon nanotubes so that the void ratio increases, introducing more air with poor thermal conductivity in the polyurethane matrix, increasing phonon scattering, and causing the appearance of the problem of reduced thermal conductivity), using aluminum nitrate as a precursor, aluminum oxide is coated on the surface of the multi-walled carbon nanotubes to prepare hybrid multi-walled carbon nanotubes.
[0040] The present invention uses carboxylated multi-walled carbon nanotubes as a matrix, and utilizes diaminodiphenyl ether and silver nitrate crystals to jointly modify the matrix to prepare silver-modified composite multi-walled carbon nanotubes containing diamino groups (the introduction of silver nanoparticles, on the one hand, can effectively limit the agglomeration of composite multi-walled carbon nanotubes containing diamino structures in a polyurethane matrix, can improve the dispersion performance of composite multi-walled carbon nanotubes with diamino structures during the curing process, can help the modified multi-walled carbon nanotube filler to be more closely bonded to the polyurethane matrix, and improve adhesion and thermal conductivity; on the other hand, similar to the previous hybrid multi-walled carbon nanotubes modified by alumina coating, can form heat conduction channels between metal nanoparticles, can greatly improve the radial heat exchange performance of multi-walled carbon nanotubes, and further improve the thermal conductivity of the heat dissipation coating).
[0041] The present invention treats hybrid multi-walled carbon nanotubes and composite multi-walled carbon nanotubes with anionic surfactants to make their surfaces negatively charged; treats expanded graphite with cationic surfactants to make its surface positively charged; and finally prepares modified multi-walled carbon nanotubes through electrostatic attraction. The introduction of expanded graphite, on the one hand, can further inhibit the agglomeration of multi-walled carbon nanotubes in a polyurethane matrix due to its own two-dimensional sheet structure; on the other hand, hybrid multi-walled carbon nanotubes and composite multi-walled carbon nanotubes can be intercalated in expanded graphite to form a similar "bridging" effect, further improving the overall thermal conductivity network of the heat dissipation coating and further improving the thermal conductivity of the heat dissipation coating. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] In the following embodiments, the multi-walled carbon nanotubes have a diameter of 10 nm and a length of 3 μm, and are purchased from Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences; the molecular weight of polyvinyl alcohol is 31000-50000, and is purchased from Chengdu Cologne Chemical Reagent Factory; solvent oil CAS: 64742-94-5; the brand of nano-silicon aluminum alloy powder is AlSi50, and is purchased from Aoke New Materials; the defoamer model is polyurethane defoamer YRXP-07B, and is purchased from Guangzhou Yourun; the nano-dispersant model is D-430, and is purchased from Xintai Chemical; the expanded graphite model is EG200, and is purchased from Shandong Shuangyu Carbon; poly(1,4-butylene adipate) diol Mn=1000, and is purchased from Aladdin Reagent Company; polyethylene glycol diglycidyl ether Mn=500, and is purchased from Sigma-Aldrich; the remaining raw materials are all commercially available.
[0044] The method for preparing carboxylated multi-walled carbon nanotubes comprises the following steps:
[0045] 5 g of multi-walled carbon nanotubes were added to a mixed solution consisting of concentrated nitric acid and concentrated hydrochloric acid in a volume ratio of 1:3, ultrasonically dispersed for 30 minutes, heated to 75°C and stirred for 24 hours, and the mixture was added to deionized water in a fume hood for dilution, precipitated, and the supernatant was removed. The operation was repeated until there was no supernatant, the precipitated mixture was centrifuged, the supernatant was removed, the precipitate was washed to pH 7, and vacuum dried at 70°C to obtain carboxylated multi-walled carbon nanotubes.
[0046] The preparation method of modified polyurethane comprises the following steps:
[0047] Ethylene glycol was added into the reaction vessel, treated at 90°C and -0.08MPa for 2h, cooled to 50°C, trimethylhexamethylene diisocyanate (a mixture of 2,2,4- and 2,4,4-) was added at a molar ratio of -NCO to -OH of 4:1, heated to 70°C and reacted for 3h to obtain modified polyurethane.
[0048] The preparation method of polyurethane modified epoxy resin comprises the following steps:
[0049] Isophorone diisocyanate and poly(1,4-butylene adipate) diol were mixed at a molar ratio of -NCO to -OH of 3:1, heated to 60°C for reaction for 2 hours to synthesize a prepolymer containing an isocyanate group end-capping, and polyethylene glycol diglycidyl ether was mixed with the prepolymer at a molar ratio of -NCO to -OH of 1.05:1 for reaction for 60 seconds to obtain a polyurethane-modified epoxy resin.
[0050] Example 1: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Add 30 g of xylene and 30 g of butyl acetate to 30 g of solvent oil, stir evenly to obtain a mixed solvent; add 10 g of multi-walled carbon nanotubes and 10 g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5 g of nano-dispersant D-430 and 0.4 g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1 hour, add 30 g of modified polyurethane and 20 g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0051] S2: Add 4 g of imidazole curing agent into a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, and stir evenly to obtain component B;
[0052] S3: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0053] Example 2: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Dissolve 2 g of polyvinyl alcohol in 100 g of N,N-dimethylformamide, add 0.5 g of carboxylated multi-walled carbon nanotubes, heat to 80°C, ultrasonically treat for 1 hour, filter using a filter membrane with a pore size of 0.45 mm to obtain a filtrate; preheat the filtrate to 80°C, add a 10 wt% aluminum nitrate aqueous solution, keep warm and stir for 2 hours, add ammonia water to a pH of 9, filter, wash, vacuum dry at 80°C, grind, and calcine at 505°C for 2 hours to obtain hybrid multi-walled carbon nanotubes;
[0054] S2: 0.2 g of silver nitrate crystals and 0.1 g of benzyl mercaptan were added to ethanol, stirred evenly, and a mixed solution consisting of 0.2 g of carboxylated multi-walled carbon nanotubes, 30 mL of N,N-dimethylformamide, 2.5 g of 4,4'-diaminodiphenyl ether, 1.5 g of dicyclohexylcarbodiimide, and 0.8 g of 4-dimethylaminopyridine was added, heated to 60°C for 4 days, centrifuged, the supernatant was removed, the precipitate was washed to pH 7, and vacuum dried at 60°C to obtain composite multi-walled carbon nanotubes;
[0055] S3: Add 0.5 g of hybrid multi-walled carbon nanotubes and 0.5 g of composite multi-walled carbon nanotubes to 1 g / L sodium dodecylbenzene sulfonate solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain negatively charged multi-walled carbon nanotubes; add 0.5 g of expanded graphite to 9 g / L hexadecyltrimethylammonium bromide solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain positively charged expanded graphite; add negatively charged multi-walled carbon nanotubes and positively charged expanded graphite to deionized water, ultrasonically treat for 30 min, filter, vacuum dry, grind to obtain modified multi-walled carbon nanotubes;
[0056] S4: Add 30g of xylene and 30g of butyl acetate to 30g of solvent oil, stir evenly to obtain a mixed solvent; add 6g of multi-walled carbon nanotubes, 4g of modified multi-walled carbon nanotubes, and 10g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5g of nano-dispersant D-430 and 0.4g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1h, add 30g of modified polyurethane and 20g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0057] S5: adding 4 g of imidazole curing agent to a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, stirring evenly to obtain component B;
[0058] S6: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0059] Example 3: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Add 30 g of xylene and 30 g of butyl acetate to 30 g of solvent oil, stir evenly to obtain a mixed solvent; add 5 g of multi-walled carbon nanotubes, 5 g of modified multi-walled carbon nanotubes, and 10 g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5 g of nano-dispersant D-430 and 0.4 g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1 hour, add 30 g of modified polyurethane and 20 g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0060] S2: Add 4 g of imidazole curing agent into a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, and stir evenly to obtain component B;
[0061] S3: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0062] Example 4: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Add 30 g of xylene and 30 g of butyl acetate to 30 g of solvent oil, stir evenly to obtain a mixed solvent; add 4 g of multi-walled carbon nanotubes, 6 g of modified multi-walled carbon nanotubes, and 10 g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5 g of nano-dispersant D-430 and 0.4 g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1 hour, add 30 g of modified polyurethane and 20 g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0063] S2: Add 4 g of imidazole curing agent into a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, and stir evenly to obtain component B;
[0064] S3: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0065] Comparative Example 1: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Add 30 g of xylene and 30 g of butyl acetate to 30 solvent oil, stir evenly to obtain a mixed solvent; add 10 g of multi-walled carbon nanotubes and 10 g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5 g of nano-dispersant D-430 and 0.4 g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1 hour, add 30 g of modified polyurethane and 20 g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0066] S2: Add 4 g of imidazole curing agent into a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, and stir evenly to obtain component B;
[0067] S3: 50g of component A and 5g of component B are mixed evenly according to a certain proportion to obtain a heat dissipation coating;
[0068] The specifications of the multi-walled carbon nanotubes are a diameter of 10 nm and a length of 30 μm.
[0069] Comparative Example 2: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Dissolve 2 g of polyvinyl alcohol in 100 g of N,N-dimethylformamide, add 0.5 g of carboxylated multi-walled carbon nanotubes, heat to 80°C, ultrasonically treat for 1 hour, filter using a filter membrane with a pore size of 0.45 mm to obtain a filtrate; preheat the filtrate to 80°C, add a 10 wt% aluminum nitrate aqueous solution, keep warm and stir for 2 hours, add ammonia water to a pH of 9, filter, wash, vacuum dry at 80°C, grind, and calcine at 505°C for 2 hours to obtain hybrid multi-walled carbon nanotubes;
[0070] S2: 0.2 g of silver nitrate crystals and 0.1 g of benzyl mercaptan were added to ethanol, stirred evenly, and a mixed solution consisting of 0.2 g of carboxylated multi-walled carbon nanotubes, 30 mL of N,N-dimethylformamide, 2.5 g of 4,4'-diaminodiphenyl ether, 1.5 g of dicyclohexylcarbodiimide, and 0.8 g of 4-dimethylaminopyridine was added, heated to 60°C for 4 days, centrifuged, the supernatant was removed, the precipitate was washed to pH 7, and vacuum dried at 60°C to obtain composite multi-walled carbon nanotubes;
[0071] S3: Add 0.5 g of hybrid multi-walled carbon nanotubes to 1 g / L sodium dodecylbenzene sulfonate solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80°C, and grind to obtain negatively charged multi-walled carbon nanotubes; add 0.5 g of composite multi-walled carbon nanotubes to 9 g / L hexadecyltrimethylammonium bromide solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80°C, and grind to obtain positively charged composite multi-walled carbon nanotubes; add negatively charged multi-walled carbon nanotubes and positively charged composite multi-walled carbon nanotubes to deionized water, ultrasonically treat for 30 min, filter, vacuum dry, and grind to obtain modified multi-walled carbon nanotubes;
[0072] S4: Add 30g of xylene and 30g of butyl acetate to 30g of solvent oil, stir evenly to obtain a mixed solvent; add 6g of multi-walled carbon nanotubes, 4g of modified multi-walled carbon nanotubes, and 10g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5g of nano-dispersant D-430 and 0.4g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1h, add 30g of modified polyurethane and 20g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0073] S5: adding 4 g of imidazole curing agent to a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, stirring evenly to obtain component B;
[0074] S6: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0075] Comparative Example 3: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Dissolve 2 g of polyvinyl alcohol in 100 g of N,N-dimethylformamide, add 0.5 g of carboxylated multi-walled carbon nanotubes, heat to 80°C, ultrasonically treat for 1 hour, filter using a filter membrane with a pore size of 0.45 mm to obtain a filtrate; preheat the filtrate to 80°C, add a 10 wt% aluminum nitrate aqueous solution, keep warm and stir for 2 hours, add ammonia water to a pH of 9, filter, wash, vacuum dry at 80°C, grind, and calcine at 505°C for 2 hours to obtain hybrid multi-walled carbon nanotubes;
[0076] S2: 0.2 g of silver nitrate crystals and 0.1 g of benzyl mercaptan were added to ethanol, stirred evenly, and a mixed solution consisting of 0.2 g of carboxylated multi-walled carbon nanotubes, 30 mL of N,N-dimethylformamide, 2.5 g of 4,4'-diaminodiphenyl ether, 1.5 g of dicyclohexylcarbodiimide, and 0.8 g of 4-dimethylaminopyridine was added, heated to 60°C for 4 days, centrifuged, the supernatant was removed, the precipitate was washed to pH 7, and vacuum dried at 60°C to obtain composite multi-walled carbon nanotubes;
[0077] S3: Add 0.5 g of hybrid multi-walled carbon nanotubes and 0.5 g of composite multi-walled carbon nanotubes to 1 g / L sodium dodecylbenzene sulfonate solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain negatively charged multi-walled carbon nanotubes; add 1 g of expanded graphite to 9 g / L hexadecyltrimethylammonium bromide solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain positively charged expanded graphite; add negatively charged multi-walled carbon nanotubes and positively charged expanded graphite to deionized water, ultrasonically treat for 30 min, filter, vacuum dry, grind to obtain modified multi-walled carbon nanotubes;
[0078] S4: Add 30g of xylene and 30g of butyl acetate to 30g of solvent oil, stir evenly to obtain a mixed solvent; add 6g of multi-walled carbon nanotubes, 4g of modified multi-walled carbon nanotubes, and 10g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5g of nano-dispersant D-430 and 0.4g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1h, add 30g of modified polyurethane and 20g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0079] S5: adding 4 g of imidazole curing agent to a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, stirring evenly to obtain component B;
[0080] S6: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0081] Comparative Example 4: A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet: S1: Dissolve 2 g of polyvinyl alcohol in 100 g of N,N-dimethylformamide, add 0.5 g of carboxylated multi-walled carbon nanotubes, heat to 80°C, keep warm and stir for 1 hour, filter using a filter membrane with a pore size of 0.45 mm to obtain a filtrate; preheat the filtrate to 80°C, add a 10 wt% aluminum nitrate aqueous solution, keep warm and stir for 2 hours, add ammonia water to a pH of 9, filter, wash, vacuum dry at 80°C, grind, and calcine at 505°C for 2 hours to obtain hybrid multi-walled carbon nanotubes;
[0082] S2: 0.2 g of silver nitrate crystals and 0.1 g of benzyl mercaptan were added to ethanol, stirred evenly, and a mixed solution consisting of 0.2 g of carboxylated multi-walled carbon nanotubes, 30 mL of N,N-dimethylformamide, 2.5 g of 4,4'-diaminodiphenyl ether, 1.5 g of dicyclohexylcarbodiimide, and 0.8 g of 4-dimethylaminopyridine was added, heated to 60°C for 4 days, centrifuged, the supernatant was removed, the precipitate was washed to pH 7, and vacuum dried at 60°C to obtain composite multi-walled carbon nanotubes;
[0083] S3: Add 0.5 g of hybrid multi-walled carbon nanotubes and 0.5 g of composite multi-walled carbon nanotubes to 1 g / L sodium dodecylbenzene sulfonate solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain negatively charged multi-walled carbon nanotubes; add 0.5 g of expanded graphite to 9 g / L hexadecyltrimethylammonium bromide solution, ultrasonically treat for 30 min, filter, wash, vacuum dry at 80 ° C, grind to obtain positively charged expanded graphite; add negatively charged multi-walled carbon nanotubes and positively charged expanded graphite to deionized water, ultrasonically treat for 30 min, filter, vacuum dry, grind to obtain modified multi-walled carbon nanotubes;
[0084] S4: Add 30g of xylene and 30g of butyl acetate to 30g of solvent oil, stir evenly to obtain a mixed solvent; add 6g of multi-walled carbon nanotubes, 4g of modified multi-walled carbon nanotubes, and 10g of nano-silicon aluminum alloy powder to the mixed solvent, stir evenly, add 5g of nano-dispersant D-430 and 0.4g of defoamer YRXP-07B, stir evenly, ultrasonically disperse for 1h, add 30g of modified polyurethane and 20g of polyurethane-modified epoxy resin, stir evenly to obtain component A;
[0085] S5: adding 4 g of imidazole curing agent to a mixed solvent consisting of 30 g of xylene, 30 g of butyl acetate and 30 g of solvent oil, stirring evenly to obtain component B;
[0086] S6: Mix 50g of component A and 5g of component B in proportion to obtain a heat dissipation coating.
[0087] Experiment: Thermal conductivity test of heat dissipation coating:
[0088] The heat dissipation coating was evenly coated on the PET film with a thickness of 50 μm. After baking and curing, it was peeled off from the PET film and cut into 20 cm × 5 cm rectangular strips. The thermal conductivity of the coating at room temperature was measured using the transient hot wire method.
[0089] Thermal coating adhesion test:
[0090] The adhesion of the coating was tested according to the ISO 2409-2007 scratch method at a test temperature of 85°C.
[0091] Table 1 Heat dissipation coating performance test data table
[0092]
[0093]
[0094] Conclusion: The heat dissipation coating prepared by the present invention has excellent adhesion and thermal conductivity.
[0095] The multi-walled carbon nanotubes used in Comparative Example 1 are too long, resulting in reduced thermal conductivity.
[0096] In Comparative Example 2, no expanded graphite was introduced, resulting in reduced dispersion performance, weakened bridging effect, and reduced thermal conductivity.
[0097] In Comparative Example 3, excessive expanded graphite is introduced. Since the thermal conductivity of expanded graphite is much lower than that of multi-walled carbon nanotubes, excessive expanded graphite reduces the heat transfer between the multi-walled carbon nanotubes, resulting in reduced thermal conductivity.
[0098] In Comparative Example 4, no ultrasonic treatment was performed during the grafting of polyvinyl alcohol, and the length of the multi-walled carbon nanotubes increased, resulting in an increase in the porosity, and more air with poor thermal conductivity was introduced into the polyurethane matrix, which increased phonon scattering and reduced thermal conductivity.
[0099] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a heat dissipation coating for the outer layer of an electrical cabinet, characterized in that: The following steps are involved: S1: Add xylene and butyl acetate to solvent oil, stir evenly to obtain a mixed solvent; add filler and nano alloy powder to the mixed solvent, stir evenly, add nano dispersant and defoamer, stir evenly, ultrasonically disperse for 1-2h, add modified polyurethane and polyurethane modified epoxy resin, stir evenly to obtain component A; S2: adding the curing agent into a mixed solvent consisting of xylene, butyl acetate and solvent oil, stirring evenly to obtain component B; S3: Mix component A and component B evenly according to a certain proportion to obtain a heat dissipation coating.
2. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The proportions of the components in the A component, by mass, are 30-50 parts of modified polyurethane, 20-40 parts of polyurethane modified epoxy resin, 5-10 parts of filler, 1-5 parts of nano-dispersant, 0.2-0.5 parts of defoamer, 10-20 parts of nano-alloy powder, 30-50 parts of solvent oil, 30-50 parts of xylene, and 30-50 parts of butyl acetate.
3. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The proportions of the components in the B component, by mass, are 1-10 parts of curing agent, 30-50 parts of xylene, 30-50 parts of butyl acetate, and 30-50 parts of solvent oil.
4. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The modified polyurethane is a hydroxyl-terminated polyurethane synthesized from aliphatic isocyanate and diol; the diol includes any one or more of ethylene glycol, butanediol, diethylene glycol, and hexanediol.
5. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The epoxy equivalent of the polyurethane modified epoxy resin is 500-700.
6. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The filler includes any one or two of multi-walled carbon nanotubes and modified multi-walled carbon nanotubes, and the multi-walled carbon nanotubes in the multi-walled carbon nanotubes and the modified multi-walled carbon nanotubes have a diameter of 10-100nm and a length of 2-3μm; the nano alloy powder includes any one or more of nano silicon aluminum alloy powder, nano silicon aluminum oxygen carbon alloy powder, and nano aluminum carbon alloy powder; the curing agent includes any one or two of imidazoles and dicyandiamide.
7. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: The mass ratio of the A component to the B component is 100:(5-20).
8. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 7, characterized in that: The method for preparing the modified multi-walled carbon nanotubes comprises the following steps: Step (1): adding multi-walled carbon nanotubes to a mixed solution of concentrated nitric acid and concentrated hydrochloric acid, ultrasonically dispersing for 30-45 minutes, heating to 75-80° C. and stirring for 24 hours, diluting the mixture in deionized water in a fume hood, precipitating, removing the supernatant, repeating the operation until there is no supernatant, centrifuging the precipitated mixed solution, removing the supernatant, washing the precipitate to a pH of 7-7.2, and vacuum drying at 60-80° C. to obtain carboxylated multi-walled carbon nanotubes; Step (2): dissolving polyvinyl alcohol in N,N-dimethylformamide, adding carboxylated multi-walled carbon nanotubes, heating to 80-85°C, ultrasonically treating for 1-1.5h, filtering using a filter membrane with a pore size of 0.4-0.45mm to obtain a filtrate; preheating the filtrate to 80-85°C, adding an aqueous solution of aluminum nitrate, keeping warm and stirring for 2-2.5h, adding ammonia water to a pH of 9-10, filtering, washing, vacuum drying at 80-85°C, grinding, and calcining at 495-505°C for 2-2.5h to obtain hybrid multi-walled carbon nanotubes; Step (3): adding silver nitrate crystals and benzyl mercaptan to ethanol, stirring evenly, adding a mixed solution consisting of carboxylated multi-walled carbon nanotubes, N,N-dimethylformamide, 4,4'-diaminodiphenyl ether, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine, heating to 60-65° C. for reaction for 4-5 days, centrifuging, removing the supernatant, washing the precipitate to a pH of 7-7.2, and vacuum drying at 60-65° C. to obtain composite multi-walled carbon nanotubes; Step (4): adding hybrid multi-walled carbon nanotubes and composite multi-walled carbon nanotubes to a sodium dodecylbenzene sulfonate solution, ultrasonically treating for 30-45 minutes, filtering, washing, vacuum drying at 80-85° C., and grinding to obtain negatively charged multi-walled carbon nanotubes; adding expanded graphite to a hexadecyltrimethylammonium bromide solution, ultrasonically treating for 30-45 minutes, filtering, washing, vacuum drying at 80-85° C., and grinding to obtain positively charged expanded graphite; adding negatively charged multi-walled carbon nanotubes and positively charged expanded graphite to deionized water, ultrasonically treating for 30-45 minutes, filtering, vacuum drying, and grinding to obtain modified multi-walled carbon nanotubes.
9. The method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to claim 1, characterized in that: In step (1), the volume ratio of concentrated nitric acid to concentrated hydrochloric acid is 1:3; in step (2), the mass fraction of polyvinyl alcohol dissolved in N,N-dimethylformamide is 2-3%, and the mass fraction of aluminum nitrate aqueous solution is 10-12%; in step (3), the molar ratio of silver nitrate crystals to benzyl mercaptan is 100:(6.7-8.4), the mass ratio of carboxylated multi-walled carbon nanotubes to 4,4'-diaminodiphenyl ether to dicyclohexylcarbodiimide to 4-dimethylaminopyridine is (1-2):(20-30):(10-18):(6-10), and the mass ratio of silver nitrate crystals to carboxylated multi-walled carbon nanotubes is 1:1; in step (4), the mass ratio of hybrid multi-walled carbon nanotubes to composite multi-walled carbon nanotubes to positively charged expanded graphite is 1:1:1, the concentration of sodium dodecylbenzenesulfonate solution is 1-2 g / L, and the concentration of hexadecyltrimethylammonium bromide solution is 9-10 g / L.
10. The heat dissipation coating prepared according to the method for preparing the heat dissipation coating for the outer layer of an electrical cabinet according to any one of claims 1 to 9.
Citation Information
Patent Citations
Carbon nano-tube coating material for refrigeration device, preparation method and applications thereof
CN110938346A
Cited By
Hybrid nanofluid, coating, liquid heat-preservation storage and transportation equipment and preparation method of liquid heat-preservation storage and transportation equipment
CN119684832A