Ceramic coating as well as preparation method and application thereof
By using polysilazane resin and sintering additives in ceramic coatings, combined with phased temperature-raising control technology, the problem of fragility of ceramic hanging baskets and sticky silk hanging baskets is solved, and the ceramic coating is realized The strong combination of the substrate and the high temperature stability and corrosion resistance of the platinum hanging basket improve the performance and safety of the hanging basket.
Patent Information
- Application Number
- CN202411057696.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing ceramic hanging baskets are fragile and costly in high temperature tests. Platinum hanging baskets are prone to sticking and hanging wires during use, which affects the accuracy of the test results and increases maintenance costs.
Using a ceramic coating formulation, including aluminum trioxide, silica, polysilazane resin, sintering aid, plasticizer and lubricant, the interface bonding and toughness are enhanced by the polysilazane resin, and through Stage heating regulation achieves viscous sintering, improving the strength of the coating and the thermal stability of the matrix.
It significantly improves the interface bonding ability between the ceramic coating and the substrate, enhances the thermal stability and durability of the platinum hanging basket, reduces the risk of coating peeling, and improves the resistance to corrosion, extends the service life of the hanging basket.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic coatings, and in particular to a ceramic coating, a preparation method and application thereof. Background Art
[0002] Ceramic coatings are often used as protective material coatings and are applied to the surface of substrates (such as hanging baskets). In the prior art, hanging baskets are mainly platinum hanging baskets or ceramic hanging baskets. For example, platinum hanging baskets are prone to sticking and hanging wires during high temperature testing, causing deformation or damage, affecting the accuracy of test results, and need to be regularly replaced or maintained during use, which increases costs and reduces efficiency. Ceramic hanging baskets are brittle and break easily during use, which also increases costs. Therefore, it is particularly important to develop a platinum hanging basket with a ceramic coating. Summary of the invention
[0003] The first object of the present invention is to provide a ceramic coating which has a strong interface bonding ability with a base material and is not easy to fall off, so that the base material exhibits excellent performance.
[0004] A second object of the present invention is to provide a platinum hanging basket with a ceramic coating, which exhibits good thermal stability and durability and has good corrosion resistance.
[0005] The embodiments of the present invention are implemented by the following technical solutions:
[0006] A ceramic coating comprises, by weight: 50-70 parts of aluminum oxide, 20-30 parts of silicon dioxide, 5-10 parts of polysilazane resin, 0.5-5 parts of sintering aid, 0.5-5 parts of plasticizer, 0.5-5 parts of lubricant and 10-20 parts of water.
[0007] The inventors found that after the ceramic slurry is coated on the hanging basket substrate, the weak interface bonding force can easily cause the coating to fall off during operation, especially in the case of rapid heating and cooling, affecting the performance of the coating. Therefore, the present invention uses polysilazane resin as a binder to achieve the purpose of toughness enhancement, and the surface coating of the sintered substrate material can improve the interface bonding ability, making it less likely to fall off, so that the performance of the substrate material is significantly improved; specifically:
[0008] Polysilazane resin has a greater deformation capacity than brittle ceramics. When the substrate is subjected to external force, the fracture generally occurs first in the internal defects of the substrate, and then gradually expands to the surface of the substrate. The presence of the coating can effectively prevent this phenomenon from occurring. And the coating containing the binder used in the present invention is only physically wrapped on the surface of the substrate, and will not chemically react with the substrate, thereby ensuring the inherent performance and stability of the substrate material; and the polysilazane resin has good fluidity and high temperature resistance. If an external force collision occurs, the surface pores can be filled and the coating is thin and uniform, which is convenient for coating, and can be converted into SiCN, SiCNO or silicon dioxide ceramic coating under high temperature conditions, which improves the strength of the substrate, and combines with the substrate interface, improves the interfacial shear strength, and improves the stress transfer effect from the substrate to the polysilazane resin, thereby improving the overall strength and energy absorption of the substrate.
[0009] Furthermore, the sintering aid includes one or more of iron oxide, calcium carbonate, magnesium oxide, potassium oxide and sodium oxide. The present invention uses the above sintering aid to adjust the adhesion, hardness and heat resistance of the ceramic and enhance the chemical corrosion resistance of the coating.
[0010] Furthermore, the plasticizer includes one or more of ethylene glycol, polyacrylate, glycerol, benzoic acid, and malonic acid ester.
[0011] Furthermore, the lubricant includes starch and glycerol.
[0012] A method for preparing a ceramic coating comprises the following steps:
[0013] S1. Aluminum oxide and silicon dioxide are mixed, wet-milled and dried to obtain a mixture;
[0014] S2. After the polysilazane resin and the mixed material are evenly mixed, vacuum degassing treatment is carried out in a vacuum drying oven at a temperature of 80-100° C. and a negative pressure of 90 kPa, and then the remaining raw materials are added, and after heating and mixing, the ceramic coating is obtained.
[0015] Furthermore, in S1, the ball-to-material mass ratio during wet grinding is 4:1, and the slurry after wet grinding is vacuum dried at 50-80°C.
[0016] Furthermore, in S1, the mixture is heated and mixed in a constant temperature water bath at 30 to 40° C. for 1 to 2 hours.
[0017] The application of the ceramic coating includes coating it on the surface of a substrate, and after curing, a substrate material coated with the ceramic coating is obtained.
[0018] Specifically, in the present invention, the ceramic coating is uniformly coated on the surface of the hanging basket, and then the platinum hanging basket with the ceramic coating is subjected to stage-by-stage temperature regulation to obtain a platinum hanging basket with a ceramic coating; specifically, when performing stage-by-stage temperature regulation: first calcine at 150-250°C for 0.5-1.5h, then calcine at 350-450°C for 0.5-1.5h, then calcine at 550-650°C for 0.5-1.5h, and finally calcine at 1000-1500°C for 0.5-1.5h, and cool to room temperature with the furnace after sintering is completed; or cool to room temperature after keeping warm for 2h in a vacuum or inert atmosphere. The present invention adopts staged temperature increase regulation. The first step of sintering is carried out at a relatively low temperature, which strengthens the viscous sintering of alumina and silicon dioxide. Through gradient temperature increase, layer-by-layer viscous sintering is achieved, thereby improving the strength of the coating and avoiding the expansion of cracks when subjected to external force. At the same time, under the protective effect of the coating, the thermal stability and durability of the substrate (such as a hanging basket) are further improved.
[0019] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0020] 1. The ceramic coating of the present invention can achieve the purpose of enhancing the toughness of the coating and the substrate. The surface coating of the sintered substrate material can improve the interface bonding ability and is not easy to fall off, so that the performance of the substrate material is significantly improved.
[0021] 2. The preparation process of the present invention adopts staged temperature control. The first step of sintering is carried out at a relatively low temperature, which strengthens the viscous sintering of alumina and silica. By increasing the temperature in a gradient, layer-by-layer viscous sintering is achieved, thereby improving the strength of the coating and avoiding the expansion of cracks when subjected to external force. At the same time, under the protective effect of the coating, the thermal stability and durability of the substrate (such as a hanging basket) are further improved. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0023] Example 1
[0024] A ceramic coating comprises, by weight: 60 parts of aluminum oxide, 25 parts of silicon dioxide, 10 parts of a polysilazane resin binder, 1 part of iron oxide, 1 part of calcium carbonate, 2 parts of ethylene glycol, 3 parts of glycerol, and 15 parts of water.
[0025] The method for preparing the ceramic coating comprises the following steps:
[0026] S1. Aluminum oxide and silicon dioxide are mixed, wet-milled and dried to obtain a mixture; the ball-to-material mass ratio during wet milling is 4:1, and the slurry after wet milling is vacuum dried at 50-80°C;
[0027] S2. After the polysilazane resin and the mixed material are uniformly mixed, vacuum degassing treatment is carried out in a vacuum drying oven at a temperature of 90°C and a negative pressure of 90 kPa, and then the remaining raw materials are added, and the mixture is mixed and stirred in a constant temperature water bath at 35°C for 2 hours to obtain the ceramic coating.
[0028] The above-mentioned ceramic coating is evenly applied to the surface of the platinum hanging basket, and then the temperature is adjusted in stages. Specifically, it is first fired at 200°C for 1 hour, then fired at 400°C for 1 hour, then fired at 600°C for 1 hour, and finally fired at 1200°C for 1 hour. After sintering, it is cooled to room temperature with the furnace to obtain a platinum hanging basket with a ceramic coating.
[0029] Example 2
[0030] The difference between this embodiment and embodiment 1 is that:
[0031] A ceramic coating comprises, by weight: 55 parts of aluminum oxide, 23 parts of silicon dioxide, 5 parts of polysilazane resin, 2 parts of magnesium oxide, 4 parts of polyacrylate, 1 part of glycerol and 20 parts of water.
[0032] Example 3
[0033] The difference between this embodiment and embodiment 1 is that:
[0034] A ceramic coating comprises, by weight: 65 parts of aluminum oxide, 27 parts of silicon dioxide, 8 parts of polysilazane resin, 4 parts of sintering aid, 1 part of plasticizer, 3 parts of lubricant and 18 parts of water.
[0035] Example 4
[0036] The difference between this embodiment and embodiment 1 is that:
[0037] A ceramic coating comprises, by weight: 66 parts of aluminum oxide, 22 parts of silicon dioxide, 6 parts of polysilazane resin, 3 parts of sintering aid, 4 parts of plasticizer, 2 parts of lubricant and 13 parts of water.
[0038] Example 5
[0039] The difference between this embodiment and embodiment 1 is that:
[0040] A ceramic coating comprises, by weight: 55 parts of aluminum oxide, 28 parts of silicon dioxide, 9 parts of polysilazane resin, 2 parts of sintering aid, 2 parts of plasticizer, 1 part of lubricant and 16 parts of water.
[0041] Comparative Example 1
[0042] The difference between this comparative example and Example 1 is that the binder is polyvinyl alcohol.
[0043] Experimental Example 1
[0044] The platinum hanging baskets prepared in the embodiments and comparative examples were subjected to performance tests, and the results are shown in Table 1. The test methods for acid corrosion and alkali corrosion are as follows: the platinum hanging baskets with ceramic coatings prepared in the embodiments and comparative examples were cut into the same size and placed in a 5wt% sulfuric acid solution and a 20wt% sodium hydroxide solution for 12 hours, and the changes on the surface of the platinum hanging baskets were observed. The wear rate of the ceramic material was measured according to JC / T848.1-1999 "Wear-Resistant Alumina Ceramic Balls", and the data were recorded after three parallel tests.
[0045] Table 1 - Test results
[0046] Is the coating peeling off? Acid corrosion Alkaline corrosion Example 1 no No spots or corrosion pits No spots or corrosion pits Example 2 no No spots or corrosion pits No spots or corrosion pits Example 3 no No spots or corrosion pits No spots or corrosion pits Example 4 no No spots or corrosion pits No spots or corrosion pits Example 5 no No spots or corrosion pits No spots or corrosion pits Comparative Example 1 Shedding A few spots and corrosion pits A few spots and corrosion pits
[0047] It can be seen from the results in Table 1 that the platinum hanging basket with ceramic coating of the present invention has a strong interface bonding ability between the ceramic coating and the platinum hanging basket and is not easy to fall off, so that the platinum hanging basket exhibits good thermal stability and durability, and has good corrosion resistance, which improves the use stability and safety of the platinum hanging basket as a whole.
[0048] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A ceramic coating, characterized in that: The composition comprises, by weight: 50-70 parts of aluminum oxide, 20-30 parts of silicon dioxide, 5-10 parts of polysilazane resin, 0.5-5 parts of sintering aid, 0.5-5 parts of plasticizer, 0.5-5 parts of lubricant and 10-20 parts of water.
2. The ceramic coating according to claim 1, characterized in that The sintering aid includes one or more of iron oxide, calcium carbonate, magnesium oxide, potassium oxide and sodium oxide.
3. The ceramic coating according to claim 1, characterized in that The plasticizer includes one or more of ethylene glycol, polyacrylate, glycerol, benzoic acid, and malonate.
4. The ceramic coating according to claim 1, characterized in that The lubricant includes starch and glycerol.
5. A method for preparing a ceramic coating according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Aluminum oxide and silicon dioxide are mixed, wet-milled and dried to obtain a mixture; S2. After the polysilazane resin and the mixed material are evenly mixed, vacuum degassing treatment is carried out in a vacuum drying oven at a temperature of 80-100° C. and a negative pressure of 90 kPa, and then the remaining raw materials are added, and after heating and mixing, the ceramic coating is obtained.
6. The method for preparing a ceramic coating according to claim 5, characterized in that: In S1, the ball-to-material mass ratio during wet grinding is 4:1, and the slurry after wet grinding is vacuum dried at 50-80°C.
7. The method for preparing a ceramic coating according to claim 5, wherein in S2, the heating and mixing is carried out in a constant temperature water bath at 30-40°C and stirred for 1-2 hours.
8. An application of a ceramic coating, characterized in that: The ceramic coating according to any one of claims 1 to 4 or the ceramic coating prepared by the preparation method according to any one of claims 5 to 7 is applied to the surface of a substrate, and after curing, a substrate material coated with the ceramic coating is obtained.
9. The use of the ceramic coating according to claim 8, characterized in that: The ceramic coating is evenly coated on the surface of the hanging basket, and then the platinum hanging basket with the ceramic coating is subjected to stage-by-stage temperature regulation to obtain a platinum hanging basket with the ceramic coating.
10. The use of the ceramic coating according to claim 9, characterized in that: When performing staged temperature control: first sinter at 150-250℃ for 0.5-1.5h, then sinter at 350-450℃ for 0.5-1.5h, then sinter at 550-650℃ for 0.5-1.5h, and finally sinter at 1000-1500℃ for 0.5-1.5h. After sintering, cool to room temperature with the furnace; or keep warm in vacuum or inert atmosphere for 2h and then cool to room temperature.
Citation Information
Patent Citations
Protective coating for inhibiting platinum bushing from being oxidized and volatilized, and manufacturing method and application thereof
CN101967313A
Method for preparing ceramic coating on surface of high-carbon steel
CN109706452A
Aluminum oxide ceramic slurry for transformer frameworks and preparation method and application method thereof
CN112094109A
Stainless steel-based inorganic non-stick coating and preparation method of stainless steel-based kitchen non-stick tool
CN115785703A
Heat-resistant insulated wire
JP1994128531A