High-performance environment-friendly waterproof coiled material and preparation method thereof

By using an aging-resistant waterproof layer and a glass fiber mesh reinforcement layer, combined with an environmentally friendly bonding layer, a high-performance environmentally friendly waterproof roll is formed, which solves the problems of aging of waterproof rolls and release of harmful substances, and achieves excellent waterproofing performance and Environmental protection.

CN118931408AInactive Publication Date: 2024-11-12JILIN YUWANG JIANNENG TECH CO LTD

Patent Information

Application Number
CN202411224052.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing waterproof coils are prone to aging and cracking after long-term use, resulting in a degradation of waterproofing performance and release harmful VOC substances during production and use, affecting the environment and human health.

Method used

Aging-resistant waterproof layer is made of polyvinyl chloride resin, thermoplastic polyurethane elastomer, nano-silica, antioxidants and ultraviolet absorbers, combined with a glass fiber mesh reinforcement layer, and butyl rubber, terpene resin, The bonding layer made of petroleum resin and calcium carbonate is combined with a fiberglass mesh fabric through an extruder to form a high-performance, environmentally friendly and waterproof coil.

Benefits of technology

It significantly improves the weather resistance, tensile strength and tear resistance of the waterproof coil material, extends its service life, ensures environmental protection, avoids the release of harmful substances, and meets modern environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931408A_ABST
    Figure CN118931408A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building materials, and provides a high-performance environment-friendly waterproof roll and a preparation method thereof.The high-performance environment-friendly waterproof roll comprises a waterproof layer, a reinforcing layer and a bonding layer which are sequentially arranged from top to bottom; the weather-resistant and aging-resistant waterproof coating has excellent weather resistance and aging resistance, can keep good waterproof performance under various environmental conditions, and prolongs the service life; the coiled material has excellent tensile strength and tearing strength, the used raw materials are all environment-friendly materials, are harmless to the environment and human health in the production and use process, and meet the modern environment-friendly requirements, the reinforcing layer is made of glass fiber mesh cloth, and the tensile strength of the coiled material is greatly improved. The tensile strength and tear resistance of the coiled material are remarkably improved, and the overall stability and reliability are enhanced; the bonding layer has good bonding performance and water resistance, it can be ensured that the coiled material and the base layer are firmly bonded, and the waterproof effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, in particular to a high-performance environmentally friendly waterproof coiled material and a preparation method thereof. Background Art

[0002] In construction projects, waterproofing membranes are an important waterproof material used to prevent water penetration and protect the structure and internal facilities of buildings. However, existing waterproofing membranes still have some shortcomings in terms of performance and environmental protection. For example, some traditional waterproofing membranes are prone to aging and cracking after long-term use, resulting in a decrease in waterproof performance. At the same time, some waterproofing membranes release harmful substances such as VOCs and other unpleasant odors during production and use, which have adverse effects on the environment and human health. At the same time, the traditional asphalt waterproofing membranes have a batching temperature of (180-200)℃ during the production process, which requires high energy consumption and produces a large amount of waste smoke and exhaust gas under high temperature conditions, which does not meet the environmental protection requirements of modern society.

[0003] To this end, those skilled in the art have proposed a high-performance environmentally friendly waterproof roll and a preparation method thereof to solve the problems raised by the background technology. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a high-performance environmentally friendly waterproof roll and a preparation method thereof, so as to solve the many deficiencies in the performance and environmental protection of the waterproof roll in the prior art. Traditional waterproof rolls are prone to aging, cracking and other problems after long-term use, resulting in a decrease in waterproof performance; at the same time, some waterproof rolls release harmful substances such as VOCs during production and use, causing adverse effects on the environment and human health.

[0005] A high-performance environmentally friendly waterproof roll material, comprising a waterproof layer, a reinforcement layer and a bonding layer arranged in sequence from top to bottom, wherein the waterproof layer isolation material is an aging-resistant isolation film, and the bonding layer isolation material is an isolation film with silicone oil;

[0006] The waterproof layer is made of the following raw materials in parts by weight: 50-70 parts of polyvinyl chloride resin, 20-30 parts of thermoplastic polyurethane elastomer, 5-10 parts of nano silicon dioxide, 1-3 parts of antioxidant, and 1-3 parts of ultraviolet absorber;

[0007] The reinforcement layer is glass fiber mesh cloth;

[0008] The bonding layer is made of the following raw materials in parts by weight: 30-40 parts of butyl rubber, 10-20 parts of terpene resin, 5-10 parts of petroleum resin and 10-20 parts of calcium carbonate.

[0009] The above-mentioned method for preparing a high-performance environmentally friendly waterproof coiled material comprises the following steps:

[0010] S1. Preparation of waterproof layer materials

[0011] Add polyvinyl chloride resin and thermoplastic polyurethane elastomer into a high-speed mixer, stir at 80-100°C for 10-15 minutes, then add nano silicon dioxide, antioxidant and ultraviolet absorber, and continue stirring for 5-10 minutes to obtain a waterproof layer material;

[0012] S2. Preparation of bonding layer materials

[0013] Add butyl rubber, terpene resin, petroleum resin and calcium carbonate into an internal mixer, and mix at 120-150° C. for 15-20 minutes to obtain a bonding layer material;

[0014] S3, Forming

[0015] The prepared waterproof layer material is extruded through an extruder, and is compounded with a glass fiber mesh cloth during the extrusion process. Then, an adhesive layer material is coated on the lower surface of the composite layer. After cooling, pulling, and winding, a high-performance environmentally friendly waterproof roll material is obtained.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The waterproof layer of the present invention uses polyvinyl chloride resin and thermoplastic polyurethane elastomer as main raw materials, and adds nano silicon dioxide, antioxidant and ultraviolet absorber, so that the waterproof layer has excellent weather resistance, aging resistance and anti-penetration, and can effectively extend the service life of the waterproof membrane;

[0018] 2. The reinforcing layer of the present invention adopts glass fiber mesh cloth, which can significantly improve the tensile strength and tear resistance of the waterproof coiled material and enhance its overall stability and reliability;

[0019] 3. The adhesive layer of the present invention uses butyl rubber, terpene resin, petroleum resin and calcium carbonate as raw materials, has good bonding performance and water resistance, can ensure the firm bonding between the waterproof coiled material and the base layer, and improve the waterproof effect;

[0020] 4. The raw materials used in the present invention are all environmentally friendly materials, which will not cause harm to the environment and human health during production and use, and meet the requirements of modern society for environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0022] Figure 1It is a schematic diagram of the structure of the high-performance environmentally friendly waterproof membrane of the present invention. DETAILED DESCRIPTION

[0023] The following examples are used to illustrate the present invention, but they are not intended to limit the scope of the present invention.

[0024] Example 1

[0025] A high-performance environmentally friendly waterproof roll material comprises a waterproof layer 1, a reinforcement layer 2 and a bonding layer 3 arranged in sequence from top to bottom, such as Figure 1 As shown;

[0026] The waterproof layer 1 is made of the following raw materials in parts by weight: 50 parts of polyvinyl chloride resin, 20 parts of thermoplastic polyurethane elastomer, 5 parts of nano silicon dioxide, 1 part of antioxidant, and 1 part of ultraviolet absorber;

[0027] The reinforcement layer 2 is a glass fiber mesh cloth;

[0028] The adhesive layer 3 is made of the following raw materials in parts by weight: 30 parts of butyl rubber, 10 parts of terpene resin, 5 parts of petroleum resin, and 10 parts of calcium carbonate.

[0029] The preparation method of high-performance environmentally friendly waterproof membrane comprises the following steps:

[0030] Step 1: Prepare waterproof layer 1 materials

[0031] Add polyvinyl chloride resin and thermoplastic polyurethane elastomer into a high-speed mixer, stir at 80° C. for 10 minutes, then add nano silicon dioxide, antioxidant and ultraviolet absorber, and continue stirring for 5 minutes to obtain a waterproof layer 1 material;

[0032] Step 2: Prepare the bonding layer 3 material

[0033] Add butyl rubber, terpene resin, petroleum resin and calcium carbonate into an internal mixer and mix at 120° C. for 15 minutes to obtain a bonding layer 3 material;

[0034] Step 3: Molding

[0035] The prepared waterproof layer 1 material is extruded through an extruder, and is compounded with the glass fiber mesh cloth during the extrusion process. Then, the adhesive layer 3 material is coated on the lower surface of the composite layer. After cooling, pulling, and winding, a high-performance environmentally friendly waterproof roll material is obtained.

[0036] Example 2

[0037] A high-performance environmentally friendly waterproof roll material, comprising a waterproof layer 1, a reinforcement layer 2 and a bonding layer 3 arranged in sequence from top to bottom;

[0038] The waterproof layer 1 is made of the following raw materials in parts by weight: 60 parts of polyvinyl chloride resin, 25 parts of thermoplastic polyurethane elastomer, 8 parts of nano silicon dioxide, 2 parts of antioxidant, and 2 parts of ultraviolet absorber;

[0039] The reinforcement layer 2 is a glass fiber mesh cloth;

[0040] The adhesive layer 3 is made of the following raw materials in parts by weight: 35 parts of butyl rubber, 15 parts of terpene resin, 8 parts of petroleum resin, and 15 parts of calcium carbonate.

[0041] The preparation method of high-performance environmentally friendly waterproof membrane comprises the following steps:

[0042] Step 1: Prepare waterproof layer 1 materials

[0043] Add polyvinyl chloride resin and thermoplastic polyurethane elastomer into a high-speed mixer, stir at 90° C. for 12 minutes, then add nano silicon dioxide, antioxidant, and ultraviolet absorber, and continue stirring for 8 minutes to obtain a waterproof layer 1 material;

[0044] Step 2: Prepare the bonding layer 3 material

[0045] Add butyl rubber, terpene resin, petroleum resin and calcium carbonate into an internal mixer and mix at 135° C. for 18 minutes to obtain a bonding layer 3 material;

[0046] Step 3: Molding

[0047] The prepared waterproof layer 1 material is extruded through an extruder, and is compounded with the glass fiber mesh cloth during the extrusion process. Then, the adhesive layer 3 material is coated on the lower surface of the composite layer. After cooling, pulling, and winding, a high-performance environmentally friendly waterproof roll material is obtained.

[0048] Example 3

[0049] A high-performance environmentally friendly waterproof roll material, comprising a waterproof layer 1, a reinforcement layer 2 and a bonding layer 3 arranged in sequence from top to bottom;

[0050] The waterproof layer 1 is made of the following raw materials in parts by weight: 70 parts of polyvinyl chloride resin, 30 parts of thermoplastic polyurethane elastomer, 10 parts of nano silicon dioxide, 3 parts of antioxidant, and 3 parts of ultraviolet absorber;

[0051] The reinforcement layer 2 is a glass fiber mesh cloth;

[0052] The adhesive layer 3 is made of the following raw materials in parts by weight: 40 parts of butyl rubber, 20 parts of terpene resin, 10 parts of petroleum resin, and 20 parts of calcium carbonate.

[0053] The preparation method of high-performance environmentally friendly waterproof membrane comprises the following steps:

[0054] Step 1: Prepare waterproof layer 1 materials

[0055] Add polyvinyl chloride resin and thermoplastic polyurethane elastomer into a high-speed mixer, stir at 100° C. for 15 minutes, then add nano silicon dioxide, antioxidant and ultraviolet absorber, and continue stirring for 10 minutes to obtain a waterproof layer 1 material;

[0056] Step 2: Prepare the bonding layer 3 material

[0057] Add butyl rubber, terpene resin, petroleum resin and calcium carbonate into an internal mixer and mix at 150° C. for 20 minutes to obtain a bonding layer 3 material;

[0058] Step 3: Molding

[0059] The prepared waterproof layer 1 material is extruded through an extruder, and is compounded with the glass fiber mesh cloth during the extrusion process. Then, the adhesive layer 3 material is coated on the lower surface of the composite layer. After cooling, pulling, and winding, a high-performance environmentally friendly waterproof roll material is obtained.

[0060] Comparative Example 1

[0061] The conventional waterproofing membrane is adopted, and its composition and preparation method are prior art.

[0062] The performance tests were conducted on the high-performance environmentally friendly waterproof membranes prepared in the above Examples 1-3 and the traditional waterproof membrane of Comparative Example 1. The test results are shown in the following table:

[0063] Performance Indicators Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength(MPa) 20.5 21.8 22.3 15.2 Elongation at break (%) 580 620 650 450 Waterproofness (0.3MPa, 30min) No leakage No leakage No leakage No leakage Aging resistance (1000h) No change No change No change There are cracks

[0064] It can be seen from the above test results that the high-performance environmentally friendly waterproof membranes prepared in Examples 1-3 of the present invention are significantly superior to traditional waterproof membranes in terms of tensile strength, elongation at break, tear strength, water impermeability and aging resistance.

[0065] From the above, it can be seen that it has excellent weather resistance and aging resistance, can maintain good waterproof performance under various environmental conditions, and extend the service life; excellent elongation at break and tear strength make the roll material have strong tensile and damage resistance. The raw materials used are all environmentally friendly materials, which are harmless to the environment and human health during production and use, and meet modern environmental protection requirements. The reinforcement layer 2 adopts glass fiber mesh cloth, which significantly improves the tensile strength and tear resistance of the roll material, and enhances the overall stability and reliability; the bonding layer 3 has good bonding performance and water resistance, which can ensure that the roll material is firmly bonded to the base layer and improve the waterproof effect.

[0066] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A high-performance environmentally friendly waterproof membrane, characterized in that: The invention comprises a waterproof layer (1), a reinforcement layer (2) and an adhesive layer (3) which are arranged in sequence from top to bottom, wherein: The waterproof layer (1) is made of the following raw materials in parts by weight: 50-70 parts of polyvinyl chloride resin, 20-30 parts of thermoplastic polyurethane elastomer, 5-10 parts of nano silicon dioxide, 1-3 parts of antioxidant, and 1-3 parts of ultraviolet absorber; The reinforcing layer (2) is a glass fiber mesh cloth; The bonding layer (3) is made of the following raw materials in parts by weight: 30-40 parts of butyl rubber, 10-20 parts of terpene resin, 5-10 parts of petroleum resin, and 10-20 parts of calcium carbonate.

2. The method for preparing a high-performance environmentally friendly waterproof coiled material according to claim 1, characterized in that: The following steps are involved: S1, adding polyvinyl chloride resin and thermoplastic polyurethane elastomer into a high-speed mixer for initial stirring, then adding nano silicon dioxide, antioxidant and ultraviolet absorber, stirring again to obtain a waterproof layer material; S2, adding butyl rubber, terpene resin, petroleum resin and calcium carbonate into an internal mixer for mixing to obtain a bonding layer material; S3. The prepared waterproof layer material is extruded through an extruder, and is compounded with a glass fiber mesh cloth during the extrusion process. Then, an adhesive layer material is coated on the lower surface of the compound layer. After cooling, pulling, and winding, a high-performance environmentally friendly waterproof roll material is obtained.

3. A method for preparing a high-performance environmentally friendly waterproof coiled material as claimed in claim 2, characterized in that: In step S1, the initial stirring is carried out at 80-100°C for 10-15 minutes.

4. A method for preparing a high-performance environmentally friendly waterproof coiled material as claimed in claim 2, characterized in that: In step S1, the stirring time is 5-10 minutes.

5. The method for preparing a high-performance environmentally friendly waterproof coiled material according to claim 2, characterized in that: In step S2, the mixing is performed at 120-150° C. for 15-20 minutes.

Citation Information

Patent Citations

  • Waterproof self-adhesive coiled material prepared from butyl rubber and preparation method of coiled material

    CN105585978A

  • TPO waterproof coiling material and spreading mode thereof

    CN110467887A

  • Inner reinforced aging-resistant polyvinyl chloride waterproof coiled material and preparation method thereof

    CN110983808A

  • High polymer self-adhesive waterproof coiled material

    CN202782045U

Cited By

  • Waterproof coiled material with good anti-aging performance and production method thereof

    CN120921765A