Heat-vulcanized primer for low-surface-energy base material and preparation method of heat-vulcanized primer

By using hot vulcanized base glue for low-surface energy substrates that synergize with preformed film and micro-corrosion technology in thermal vulcanized bonding technology, the problem of bonding failure on low-surface energy substrates is solved, and difficult to stick to The effective bonding of the substrate and the reduction of defective rate improves adhesion and cohesion, and extends the storage period of the base glue.

CN118931430APending Publication Date: 2024-11-12SHANGHAI TONTEE NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174768.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing thermal vulcanized adhesive bonding technology has problems with bond failure on low-surface energy substrates, especially the M-type failure type has high failure efficiency, resulting in high defect rate in production and difficult to trace specific processes. The existing avoidance method Complex and irreversible damage to rubber.

Method used

Thermal vulcanized base glue for low-surface energy substrates is used to improve the adhesion ability of the adhesive through synergistic effect of preformed film and microcorrosion technology, including the use of 2-15% halogen-containing polymer and 1-10% phenolic polymer , 1-10% nitrogen-containing monomer and/or prepolymer, 1-10% filler, 0-3% coacid and 0.1-3.0% silane modifier, prepared in combination with solvent to form suitable wetting and reaction sites point, enhance adhesion and cohesion.

Benefits of technology

Without post-processing and complex processes, the batch defective rate is effectively reduced, the adhesive performance of difficult-to-adhesive substrates is improved, the adhesion and cohesion are enhanced, and the storage period and application performance of the base glue are extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure BDA0005010417010000051
    Figure BDA0005010417010000051
Patent Text Reader

Abstract

The invention relates to the technical field of C09J123 / 00, in particular to a heat-vulcanized primer for a low-surface-energy base material and a preparation method thereof.The heat-vulcanized primer is at least prepared from, by mass, 2-15% of halogen-containing polymer, 1-10% of phenolic polymer, 1-10% of nitrogen-containing monomer and / or nitrogen-containing prepolymer, 1-10% of filler, 0-3% of auxiliary acid, 0.1-3.0% of silane modifier and the balance solvent; according to the invention, through the synergistic cooperation of the pre-film-forming technology and the micro-corrosion technology, the adhesive ability of the heat-vulcanized adhesive primer to the base material difficult to adhere is improved, the batch defective rate is reduced, and the effective adhesion of the base material difficult to adhere is realized on the basis of no need of post-treatment and complex treatment process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of C09J123 / 00, in particular to a heat-vulcanized primer for a low-surface-energy substrate and a preparation method thereof. Background Art

[0002] Rubber-metal bonding has been developed for nearly a century. The high stiffness of the substrate combined with the low stiffness of the rubber can form better shock absorption and noise reduction functions. However, the rubber system is complex and the metal surface treatment processes are numerous. These factors lead to occasional failure of rubber-metal bonding. The common failure types of rubber / metal hot vulcanization bonding are mainly the following seven categories: (1) Damage between primer adhesive and metal (MC type, abbreviated as M damage); (2) Internal damage of the adhesive primer (P type); (3) Damage between the topcoat adhesive and the primer adhesive (CP type); (4) Internal damage of the adhesive primer (C type); (5) Damage between rubber and topcoat adhesive (RC type); (6) Internal damage of rubber (R type); (7) Mixed damage, that is, two or more of the above situations occur at the same time. According to rough statistics, the current industrial damage form is mainly RC type damage, accounting for about 70%, M type damage accounts for about 25%, and other types of damage account for about 5%;

[0003] In NVH (automotive noise reduction) parts that require bonding, once the probability of the above-mentioned damage is greater than 0.01%, the manufacturer will face the problem of high compensation, ranging from hundreds of thousands to millions. The existing avoidance methods include checking the finish of the substrate treatment, regularly checking the thickness of the adhesive film, checking the feeding system, online parallax recognition, etc. However, to this day, M-type damage caused by surface treatment still occurs in mass production of auto parts manufacturers. Even with the use of advanced industrial diagnostic methods, it is difficult to accurately trace the specific process, and only a general direction can be given, which may often be verified to be no problem; for the primer of hot vulcanized adhesive, specifically, ordinary iron and steel parts are easy to bond to the primer. For example, a Chinese patent (authorization announcement number is CN101497773B) discloses a primer adhesive for hot vulcanization bonding and a preparation method thereof, which is mainly used for hot vulcanization bonding between polar / non-polar rubber and non-metal or composite materials. With the increasing requirements for corrosion protection, the bonding of some special parts has emerged, such as some materials with low surface energy (surface dyne value <32), such as carburized steel, nickel-plated parts, fiber reinforced composites (FRP), etc. The failure rate of M-type damage of such materials will be greatly increased. Manufacturers with more mature technology will adopt complex processes to solve this problem, while some manufacturers with weaker technology usually adopt post-processing methods to meet the corresponding needs, such as hot-dip galvanizing or electro-galvanizing. However, such post-processing will cause irreversible damage to the rubber due to high temperature or high current. Therefore, how to achieve adhesion on low surface dyne value surfaces while avoiding the above problems has important practical research significance. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a heat-vulcanized primer for low surface energy substrates, which improves the adhesion ability of the heat-vulcanized adhesive primer to difficult-to-bond substrates and reduces the batch defective rate through the synergistic effect of pre-filming and micro-etching technology, thereby achieving effective bonding of difficult-to-bond substrates without the need for post-processing and complicated processing techniques.

[0005] On one hand, the present invention provides a heat-vulcanized primer for a low surface energy substrate. The raw materials for its preparation include at least 2-15% of a halogen-containing polymer, 1-10% of a phenolic polymer, 1-10% of a nitrogen-containing monomer and / or a nitrogen-containing prepolymer, 1-10% of a filler, 0-3% of an auxiliary acid, 0.1-3.0% of a silane modifier, and the balance is made up of a solvent, by weight percentage.

[0006] As a preferred technical solution, the addition amount of the halogen-containing polymer is 3-10wt%, preferably 5-10wt%. The halogen-containing polymer is selected from at least one of chlorosulfonated polyethylene, chlorinated natural rubber, chlorinated polypropylene, maleic anhydride-modified chlorinated polypropylene, epoxy resin-modified chlorinated polypropylene, chlorinated ethylene vinyl acetate copolymer, and chlorinated polyethylene, preferably a combination of chlorosulfonated polyethylene and chlorinated natural rubber, and the mass ratio of the chlorosulfonated polyethylene to the chlorinated natural rubber is (1-3):1.

[0007] As a preferred technical solution, the addition amount of the phenolic polymer is 3-9wt%, preferably 4-6wt%. The phenolic polymer is a polymer of formaldehyde, phenol and cresol, preferably *PR-14170 of Sumitomo Bakelite, RT-3 series resin of Shengquan or RA-7 series resin of Tongcheng New Materials.

[0008] As a preferred technical solution, the amount of the nitrogen-containing monomer added is 1-4wt%, preferably 1.5-3wt%. The nitrogen-containing monomer is one or a combination of N,N'-m-phenylene bismaleimide, N,N'-4,4'-diphenylmethane bismaleimide, 1,11-bis(maleimido)-3,6,9-trioxaundecane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and 1,2-bismaleimidoethane. The nitrogen-containing prepolymer is a prepolymer of at least one of N,N'-m-phenylene bismaleimide, N,N'-4,4'-diphenylmethane bismaleimide, 1,11-bis(maleimido)-3,6,9-trioxaundecane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane and 1,2-bismaleimidoethane.

[0009] Preferably, the nitrogen-containing monomer is N,N'-4,4'-diphenylmethane bismaleimide.

[0010] As a preferred technical solution, the addition amount of the nitrogen-containing prepolymer is 1-4wt%, preferably 1.5-3wt%. The nitrogen-containing prepolymer is a prepolymer of at least one of N,N'-m-phenylene bismaleimide, N,N'-4,4'-diphenylmethane bismaleimide, 1,11-bis(maleimido)-3,6,9-trioxaundecane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and 1,2-bismaleimidoethane.

[0011] Preferably, the number average molecular weight of the nitrogen-containing prepolymer is 350-20,000, preferably 350-9,000, and more preferably 1,000-5,000.

[0012] Preferably, the nitrogen-containing prepolymer is a prepolymer of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, with a number average molecular weight of 1000-3000 and a dispersion index of 2-3.

[0013] The nitrogen-containing prepolymer in the present invention is prepared by using a pre-film forming technology, which specifically refers to obtaining the nitrogen-containing prepolymer after forming a film of the nitrogen-containing monomer.

[0014] In the bonding process, if you want to form good infiltration with the substrate first, the existing material bonding usually requires grinding the material to achieve the dispersion and processing of the glue. The present invention prepares the nitrogen-containing prepolymer through the pre-filming technology, and adds the nitrogen-containing monomer to the adhesive after filming, so that the provided adhesive is easier to infiltrate and form a film on the surface of the substrate to form a microscopic adhesion effect. The inventor found in the process of exploration that, in particular, the introduction of the prepolymer of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane enables the provided heat-vulcanized primer to achieve bonding between metal and EPDM rubber and butyl rubber.

[0015] As a preferred technical solution, the filler is added in an amount of 5-8wt%. The filler is selected from at least one of carbon black, silica, titanium dioxide, fly ash, and mica powder; preferably a combination of carbon black, silica, and titanium dioxide. Preferably, the mass ratio of carbon black, silica, and titanium dioxide is (1-3): (0.5-1): (2-5).

[0016] The invention reduces the cost and adjusts the thixotropy by introducing carbon black, gas silicon and titanium dioxide, so that the provided heat-vulcanized base rubber has good processability.

[0017] As a preferred technical solution, the amount of the auxiliary acid added is 0.1-0.5wt%, preferably 0.2-0.3wt%. The auxiliary acid is one or more of boric acid, 4-(trifluoromethoxy)phenylboric acid, 3-fluorophenylboric acid, and 4-phenoxyphenylboric acid; preferably, the auxiliary acid is 3-fluorophenylboric acid or 4-(trifluoromethoxy)phenylboric acid.

[0018] As a preferred technical solution, the addition amount of the silane modifier is 0.1-1.5wt%, preferably 0.2-0.3wt%. The silane modifier is selected from at least one of KH560 (γ-glycidyloxypropyl trimethoxysilane), KH570 (γ-methacryloxypropyl trimethoxysilane), γ-chloropropyl trichlorosilane, WD-31 (3-chloropropyl triethoxysilane, CAS No.: 2530-87-2), WD-62 (3-glycidyloxypropyl trimethoxysilane, CAS No.: 2602-34-8), and Si-69 (bis-[γ-(triethoxysilyl)propyl] tetrasulfide), preferably γ-chloropropyl trichlorosilane.

[0019] The invention introduces auxiliary acid and silane modifier to form Bronsted acid-base pair with halogen-containing polymer in the system, thereby improving the wettability and reaction sites of the heat-vulcanized primer to the substrate, thereby enhancing the adhesion and cohesion to the substrate. In particular, the addition amount of auxiliary acid is controlled to be 0.1-0.2wt%, which can form micro-corrosion and play a role in enhancing cohesion and bonding.

[0020] As a preferred technical solution, the solvent is methyl isobutyl ketone.

[0021] As a preferred technical solution, the parameters of the heat-vulcanized primer for the low surface energy substrate are as follows:

[0022] (1) Appearance: dark grey liquid;

[0023] (2) Viscosity, cps @ 25 °C, rotor #2, 30 rpm: 80-165;

[0024] (3) Density: 935-980, kg / m3;

[0025] (4) Solid content: 20-30wt%;

[0026] (5) Flash point: 22-24, ℃.

[0027] Another aspect of the present invention provides a method for preparing a heat-vulcanized primer for a low surface energy substrate, comprising at least the following steps:

[0028] (1) mixing 40-60 wt % of a solvent with a halogen-containing polymer and a phenolic polymer to obtain a mixed material 1;

[0029] (2) mixing the remaining solvent with the nitrogen-containing monomer and / or nitrogen-containing prepolymer, filler, auxiliary acid, and silane modifier to obtain a mixed material 2;

[0030] (3) Mixed material 1 and mixed material 2 are mixed and dispersed at a dispersion speed of 400-1000 r / min for 2-3 hours, and then ground to a material fineness of ≤45 μm to obtain the material.

[0031] As a preferred technical solution, the grinding instrument is a horizontal grinder, the grinding speed is 2000-4000rpm, the grinding medium is 0.8-1.0mm zirconium beads, the zirconium bead filling rate is 40-60%, the total grinding time is 40-60min, and the total grinding times are 2-3 times.

[0032] Beneficial Effects

[0033] 1. The present invention provides a heat-vulcanized primer for low surface energy substrates, which improves the adhesion ability of the heat-vulcanized adhesive primer to difficult-to-bond substrates by synergistically cooperating with pre-filming and micro-etching technology, reduces the batch defective rate, and realizes effective bonding of difficult-to-bond substrates without the need for post-processing and complex processing technology.

[0034] 2. The present invention prepares nitrogen-containing prepolymers through pre-filming technology, and adds nitrogen-containing monomers to adhesives after filming, so that the provided adhesive is easier to infiltrate and form films on the surface of the substrate, forming a microscopic adhesion effect.

[0035] 3. The present invention introduces auxiliary acid in combination with silane modifier to form Bronsted acid-base pair with halogen-containing polymer in the system, thereby improving the wettability and reaction sites of the heat-vulcanized primer to the substrate, thereby enhancing the adhesion and cohesion to the substrate.

[0036] 4. The present invention controls the addition amount of auxiliary acid to 0.1-0.2wt%, which can form micro-corrosion and enhance cohesion and adhesion.

[0037] 5. The introduction of nitrogen-containing prepolymer and auxiliary acid into the heat-vulcanized primer for low surface energy substrates provided by the present invention has no negative impact and helps to improve the storage period and application performance of the primer. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a physical picture of the test piece: T2 steel plate-primer-topcoat-rubber.

[0039] Figure 2 This is a real picture of the three-piece insert bushing. DETAILED DESCRIPTION

[0040] Examples 1-13

[0041] On the one hand, Examples 1-13 of the present invention provide a heat-vulcanized primer for a low surface energy substrate. The raw materials for its preparation are shown in Table 1 in terms of mass percentage.

[0042] Table 1

[0043]

[0044]

[0045] In Table 1:

[0046] The halogen-containing polymer is a combination of chlorosulfonated polyethylene and chlorinated natural rubber, and the mass ratio of the chlorosulfonated polyethylene to the chlorinated natural rubber is 2:1.

[0047] Phenolic polymers are polymers of formaldehyde, phenol and cresol, specifically Sumitomo Bakelite's *PR-14170.

[0048] The nitrogen-containing monomer is N,N'-4,4'-diphenylmethane bismaleimide.

[0049] The nitrogen-containing prepolymer is a prepolymer of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and has a number average molecular weight of 1950±50 and a dispersion index of 2.8.

[0050] The filler is a combination of carbon black, silica and titanium dioxide, and the mass ratio of the carbon black, silica and titanium dioxide is 2:0.5:4.

[0051] The auxiliary acid is 3-fluorophenylboronic acid or 4-(trifluoromethoxy)phenylboronic acid.

[0052] The silane modifier was γ-chloropropyltrichlorosilane.

[0053] The solvent is methyl isobutyl ketone

[0054] On the other hand, embodiments 1-13 of the present invention provide a method for preparing a heat-vulcanized primer for a low surface energy substrate, comprising the following steps:

[0055] (1) mixing 50 wt % of a solvent with a halogen-containing polymer and a phenolic polymer to obtain a mixed material 1;

[0056] (2) mixing the remaining solvent with the nitrogen-containing monomer and / or nitrogen-containing prepolymer, filler, auxiliary acid, and silane modifier to obtain a mixed material 2;

[0057] (3) Mixed material 1 and mixed material 2 are mixed and dispersed at a dispersion speed of 600 r / min for 2-3 hours, and then ground to a material fineness of 40 μm to obtain the material.

[0058] The grinding instrument is a horizontal grinder, the grinding speed is 3000 rpm, the grinding medium is 0.8-1.0 mm zirconium beads, the zirconium bead filling rate is 50%, the total grinding time is 40 minutes, and the total number of grinding times is 3 times.

[0059] Performance Testing

[0060] 1. The heat-vulcanized primer provided in the embodiment was tested for the various properties in Table 3. The test substrates were metal (T2 steel plate) and rubber, the topcoat was Polyton 829GB, and the coating requirements were: primer thickness 10±2μm, total thickness 30±2μm. The rubber formula is shown in Table 2, and the injection process: time 30s, feed pressure 160kg / cm 2 The rubber curing conditions are: injection vulcanization at 160°C in the cavity for 7 minutes, molding pressure of 16MPa, and molding shape of 3mm sheet (test piece: T2 steel plate-primer-topcoat-rubber, see Figure 1 ). The test method is as follows, and the test results are shown in Table 3.

[0061] (1) Conventional pressure stripping: refer to the German Volkswagen standard PV3378 bild7, test 64 samples and take the average value of the results.

[0062] (2) Thermal shock: After being kept at 150°C for one hour, 64 samples were tested by pressure release at 150°C in a high temperature test chamber. The results were averaged.

[0063] (3) Water boiling resistance test: A cut was made on the edge of the bushing and the bushing was boiled in a constant pressure water bath at 96°C for 500 h. 64 samples were tested and the results were averaged.

[0064] (4) Heat aging: The glue was stored at 50°C in a closed container for 42 days, which is approximately equivalent to one year in actual conditions. After aging for 42 days, the adhesion was tested and the product was directly pressed off. At the same time, the viscosity of the product was tested (using GB / T 10247-2008, method D, and rotational viscometer method). 64 samples were tested and the results were averaged. The viscosity of the product before and after heat aging is shown in Table 4.

[0065] Table 2

[0066] raw material Weight raw material Weight Natural rubber 90 Carbon Black N326 35 Butadiene rubber 10 Carbon Black N550 20 Zinc Oxide 4 Sulfur 2.2 Stearic acid 1.5 Accelerator M 0.5 Antioxidant 4010NA 1.5 Accelerator DM 0.8 Antioxidant D 0.5 Accelerator CZ 1.2 Gumalon 3 Accelerator TT 0.2

[0067] Table 3

[0068]

[0069]

[0070] By comparing the results in Table 3, it can be found that the introduction of nitrogen-containing prepolymers in Examples 2 and 3 relative to Example 1 has a certain adhesion-promoting effect on difficult-to-bond substrates, especially a significant improvement in the force value and a slight improvement in the adhesive rate. The possible reason for this is that the introduced nitrogen-containing prepolymers enhance the wettability and film-forming properties at the vulcanization temperature.

[0071] In Examples 5 and 6, compared with Examples 4 and 7 and 8, the amount of the silane modifier introduced is controlled at 0.2-0.3 wt % to ensure the adhesive rate and force value.

[0072] In Examples 10 and 11, compared with Examples 9 and 12 and 13, the amount of auxiliary acid introduced is controlled at 0.2-0.3 wt % to ensure the adhesive rate and strength value.

[0073] Table 4

[0074]

[0075]

[0076] Analyzing the test results in Table 4, the viscosity of the products of Examples 1-13 before and after aging is within the product definition range.

[0077] 2. The hot-vulcanized primers provided in Examples 1, 7, and 10 were used to produce 1,600 three-piece insert bushings using different substrates. The bushing test time was within 16 hours to 14 days after vulcanization. Substrate: three-piece insert bushing, see Table 5 for the material, outer tube φ46.3 mm, thickness 1.8 mm, inner rod φ23.7 mm, insert outer φ32.0 mm, thickness 1.8 mm, see Table 5 for the statistical results.

[0078] Table 5

[0079]

Claims

1. A heat-vulcanized primer for a low surface energy substrate, characterized in that: The raw materials for its preparation include at least 2-15% halogen-containing polymer, 1-10% phenolic polymer, 1-10% nitrogen-containing monomer and / or nitrogen-containing prepolymer, 1-10% filler, 0-3% auxiliary acid, 0.1-3.0% silane modifier, and the balance is made up of solvent.

2. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The halogen-containing polymer is added in an amount of 3-10wt%, and the halogen-containing polymer is selected from at least one of chlorosulfonated polyethylene, chlorinated natural rubber, chlorinated polypropylene, maleic anhydride-modified chlorinated polypropylene, epoxy resin-modified chlorinated polypropylene, chlorinated ethylene vinyl acetate copolymer, and chlorinated polyethylene.

3. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the phenolic polymer is 3-9wt%, and the phenolic polymer is a polymer of formaldehyde, phenol and cresol.

4. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the nitrogen-containing monomer is 1-4wt%, and the nitrogen-containing monomer is one or a combination of N,N'-m-phenylene bismaleimide, N,N'-4,4'-diphenylmethane bismaleimide, 1,11-bis(maleimido)-3,6,9-trioxaundecane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and 1,2-dimaleimidoethane.

5. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the nitrogen-containing prepolymer is 1-4wt%, and the nitrogen-containing prepolymer is a prepolymer of at least one of N,N'-m-phenylene bismaleimide, N,N'-4,4'-diphenylmethane bismaleimide, 1,11-bis(maleimido)-3,6,9-trioxaundecane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and 1,2-dimaleimidoethane.

6. The heat-vulcanized primer for low surface energy substrate according to claim 5, characterized in that: The number average molecular weight of the nitrogen-containing prepolymer is 350-20000.

7. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the filler is 5-8wt%, and the filler is selected from at least one of carbon black, silica, titanium dioxide, fly ash, and mica powder.

8. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the auxiliary acid is 0.1-0.5wt%, and the auxiliary acid is one or more of boric acid, 4-(trifluoromethoxy)phenylboric acid, 3-fluorophenylboric acid, and 4-phenoxyphenylboric acid.

9. The heat-vulcanized primer for low surface energy substrate according to claim 1, characterized in that: The addition amount of the silane modifier is 0.1-1.5wt%, and the silane modifier is selected from at least one of KH560, KH570, γ-chloropropyltrichlorosilane, WD-31, WD-62, and Si-69.

10. A method for preparing a heat-vulcanized primer for a low surface energy substrate according to any one of claims 1 to 9, characterized in that: At least the following steps are included: (1) mixing 40-60 wt % of a solvent with a halogen-containing polymer and a phenolic polymer to obtain a mixed material 1; (2) mixing the remaining solvent with the nitrogen-containing monomer and / or nitrogen-containing prepolymer, filler, auxiliary acid, and silane modifier to obtain a mixed material 2; (3) Mixed material 1 and mixed material 2 are mixed and dispersed at a dispersion speed of 400-1000 r / min for 2-3 hours, and then ground to a material fineness of ≤45 μm to obtain the material.