High-water-tightness submarine cable sealant capable of being crosslinked at room temperature as well as preparation method and application of high-water-tightness submarine cable sealant

By adopting a two-component system and a specific crosslinking network structure in the submarine cable sealant, the problem of insufficient watertightness and temperature resistance in complex marine environments is solved, and efficient room temperature crosslinking and stability are achieved , improving the safety and reliability of the submarine cable system.

CN118931477APending Publication Date: 2024-11-12HUBEI UNION-FIBER NEW MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411107930.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing submarine cable sealants exhibit insufficient watertightness, high crosslinking temperature, poor temperature resistance and poor extrusion in complex marine environments, limiting the safety and reliability of submarine cable systems.

Method used

Develop a high watertight room temperature crosslinked submarine cable sealant, using a two-component system, in which components A include polymethylsiloxane, hydroxysiloxane rubber, methylphenyl vinyl silicone and acrylate Allyl silicone resin, component B includes polymethylsiloxane, butyltin catalyst, antioxidant and 3-glycidyl etheroxypropyl triethoxy silicone oil, formed by fine ratio and catalyst action Stable three-dimensional cross-linking network structure.

Benefits of technology

Achieve rapid and controllable crosslinking reactions under room temperature conditions, improve the watertightness, chemical stability and mechanical strength of the sealant, maintain stability at 700 atmospheres, simplify production processes, and reduce construction costs and time. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991346550000131
    Figure BDA0004991346550000131
  • Figure BDA0004991346550000141
    Figure BDA0004991346550000141
  • Figure BDA0004991346550000171
    Figure BDA0004991346550000171
Patent Text Reader

Abstract

The invention discloses a high-water-tightness submarine cable sealant capable of being crosslinked at room temperature, a preparation method and application. The sealant is prepared from the following raw materials in parts by weight: the component A is prepared from the following raw materials in parts by weight: 120 to 150 parts of polymethylsiloxane; 35 to 50 parts of hydroxyl siloxane rubber; 60 to 80 parts of methyl phenyl vinyl silicone resin; 30 to 40 parts of acrylic acid esterified allyl organic silicon resin; 45-75 parts of a dispersant; 5-10 parts of fumed silica; 25 to 50 parts of water-absorbent resin; the component B is prepared from the following raw materials in parts by weight: 30 to 50 parts of polymethylsiloxane; 0.3 to 0.5 part of a butyl tin catalyst; 2-6 parts of an antioxidant; 2-5 parts of fumed silica; and 10 to 15 parts of 1, 3-glycidyl ether oxypropyl triethoxy silicone oil. The high-water-tightness submarine cable sealant capable of being crosslinked at room temperature provided by the invention has the advantages of high water tightness, strong aging resistance and better compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of submarine cable sealing, and in particular to a highly watertight submarine cable sealant capable of cross-linking at room temperature, a preparation method and an application thereof. Background Art

[0002] As a key material to ensure the sealing performance of marine engineering cables and their joints and terminals, the quality of submarine cable sealants is directly related to the safe and stable operation of the entire submarine cable system. This type of sealant is mainly used to fill the internal gaps of submarine cables and submarine optical cables. Therefore, it is not only necessary to have good filling convenience, but also to have excellent extrusion properties to ensure efficient and convenient construction. However, there are some limitations in the current submarine cable sealants on the market, such as insufficient watertightness, high cross-linking temperature, poor temperature resistance and inconvenience in use. These factors limit their application in complex and changeable marine environments. In particular, the problem of poor extrusion can lead to greater operational difficulties during actual construction. In view of this, it is particularly important to develop a new type of submarine cable sealant-this sealant needs to have excellent extrusion properties, can achieve a controllable rate of cross-linking reaction at room temperature, and at the same time have excellent watertightness and high temperature resistance, which is of great significance to improving the overall reliability and adaptability of submarine cable production and operation systems. Summary of the invention

[0003] In order to solve at least one of the above technical problems, a sealant with high watertightness, low cross-linking temperature, controllable cross-linking time, strong compressive strength and high temperature resistance is developed. The present application provides a high watertightness room temperature cross-linkable submarine cable sealant, a preparation method and application.

[0004] In a first aspect, the present application provides a highly watertight room temperature cross-linkable submarine cable sealant, the sealant comprising component A and component B in parts by weight; The A component includes the following raw materials by weight: 120-150 parts of polymethylsiloxane; 35-50 parts of hydroxy silicone rubber; 60-80 parts of methylphenyl vinyl silicone resin; 30-40 parts of acrylated allyl silicone resin; Dispersant 45-75 parts; 5-10 parts of fumed silica; 25-50 parts of water-absorbing resin; The B component includes the following raw materials by weight: 30-50 parts of polymethylsiloxane; 0.3-0.5 parts of butyl tin catalyst; 2-6 parts of antioxidant; 2-5 parts of fumed silica; 3-glycidyl ether oxypropyl triethoxy silicone oil 10-15 parts.

[0005] By adopting the above technical scheme, the high watertightness cross-linkable submarine cable sealant provided by the present application is aimed at the special needs of submarine cables and submarine optical cables, especially under extreme conditions of bearing pressures above 500 atmospheres, and shows excellent waterproof sealing performance. The sealant can not only delay solidification at room temperature, facilitate cable production filling, simplify the production process, and improve production efficiency, but also effectively improve the watertightness, chemical stability and mechanical strength of the sealant through its unique A component and B component design, as well as the carefully adjusted component ratio, and provide high watertightness and pressure resistance for the safe operation of submarine cable production and operation systems in extreme deep sea environments. The sealant forms a rubber-like elastomer after curing, which can withstand extreme pressures of up to 700 atmospheres (equivalent to 700 meters of seawater depth), ensures the integrity of the optical cable in the deep sea environment, effectively prevents seawater penetration, and ensures the stability of the signal transmission inside the cable and the safety of the power supply. Even under high pressure, the sealant does not flow, does not flow, and is not squeezed out, maintaining the stability and integrity of the structure. In addition, the sealant can be filled in the gap between steel wires or metal pipes under pressure at room temperature without the need for additional heating, which greatly facilitates production and improves production efficiency. After curing, it exhibits a certain rubber elasticity, which is particularly suitable for the complex environment of submarine cable laying, reducing the dependence on special equipment and reducing construction costs and time. The high watertightness and room temperature cross-linkable submarine cable sealant provided by the present application is unique in that it adopts a two-component design of component A and component B, wherein component A contains multiple key components such as polymethylsiloxane, hydroxysilicone rubber, methylphenyl vinyl silicone resin, acrylated allyl silicone resin, etc., while component B contains polymethylsiloxane, butyl tin catalyst, antioxidant, fumed silica and 3-glycidyloxypropyl triethoxy silicone oil. Through careful proportioning and design, the sealant of the present application not only realizes slow crosslinking at room temperature and room temperature controllable curing during cable placement, but also significantly outperforms conventional crosslinker systems in terms of curing rate and crosslinking reaction speed, which is mainly due to the following technical features: After the raw materials contained in component A are mixed in a specific proportion, they can quickly respond to the catalyst in component B to form a three-dimensional crosslinked network structure with excellent performance. Among them, polymethylsiloxane, as a base polymer, provides good flexibility and thermal stability. It itself also directly participates in the crosslinking reaction, and its chain segments play a skeleton role in the crosslinked network, enhancing the overall performance of the material. The hydroxyl group (-OH) in the hydroxysiloxane rubber can react with the active groups in other raw materials under the action of the catalyst to form Si-O-Si bonds and promote the construction of the crosslinked network. Its addition increases the adhesion and weather resistance of the material. Under the action of the catalyst, the vinyl of the methylphenyl vinyl silicone resin reacts with the acrylic double bond functional group in the acrylated allyl silicone resin through free radical polymerization to form a CC bond crosslinking structure, thereby strengthening the crosslinked network.The acrylic acid unsaturated bond functional group of the acrylated allyl silicone resin can also react with the hydroxyl group of the hydroxyl siloxane rubber and the vinyl group of the methylphenyl vinyl silicone resin to form CC bonds and ether bonds, thereby enhancing the stability of the cross-linked network. In addition, the present application introduces fumed silica and water-absorbing resin into component A, so that the high water-tightness room temperature cross-linkable submarine cable sealant can achieve a significant improvement in performance. Among them, fumed silica, with its high dispersibility and large specific surface area, can not only significantly enhance the mechanical strength of the sealant, improve its tear resistance and tensile strength, but also participate in the cross-linking reaction through the hydroxyl groups on its surface, increase the cross-linking density, thereby further improving the physical stability and durability of the material. In addition, the addition of fumed silica can also improve the thixotropy of the sealant, making the material easier to operate during construction, and can be better filled into various complex shapes of gaps, ensuring a good sealing effect. When the water-absorbing resin comes into contact with moisture, this type of resin can quickly absorb water and swell, effectively blocking any tiny pores or cracks, and significantly enhancing the water tightness of the material. This feature is particularly important for deep-sea environments. It can respond to seawater penetration immediately and form an effective waterproof barrier through its own expansion, effectively preventing further water intrusion and improving the anti-corrosion ability and long-term stability of the sealant. In key parts such as deep-sea cable joints and terminals, this function of the water-absorbing resin can significantly extend the service life of the submarine cable system, reduce maintenance frequency, and reduce operating costs.

[0006] While the polymethylsiloxane in component B acts as a medium, it improves the lubricity and demoulding properties of the sealant with 3-glycidyloxypropyl triethoxy silicone oil, and its good chemical stability and weather resistance also help to improve the long-term performance of the sealant. At the same time, it reacts with hydroxysiloxane rubber under the action of the catalyst butyl tin catalyst. The catalyst is a trigger for the cross-linking reaction, which can accelerate the cross-linking reaction so that the sealant can be quickly cured at room temperature. The antioxidant protects the sealant from oxidative damage, improves the long-term stability and service life of the material, especially in the marine environment, and can effectively prevent the material from aging. The present application separately adds polymethylsiloxane and fumed silica to component A and component B, respectively, in order to better control the cross-linking reaction. The present application divides the polymethylsiloxane into two parts, one part in component A and the other part in component B, and starts the cross-linking reaction by mixing component A and component B. This design helps to control the speed and degree of the cross-linking reaction, ensuring that a controllable curing process can be carried out at room temperature. Additionally, adding the polymethylsiloxane separately ensures that the sealant has a longer working time before mixing, allowing construction workers to perform filling operations without having to worry about premature curing.

[0007] The present application adds a portion of fumed silica to component A and another portion to component B, which can further optimize thixotropy after mixing and ensure that the material is smoother when filling into complex-shaped gaps. The hydroxyl groups (-OH) on the surface of fumed silica can participate in the cross-linking reaction and increase the density of the cross-linked network. Through the interaction between the fumed silica in components A and B, the stability of the cross-linked network can be further improved, thereby enhancing the physical properties of the sealant.

[0008] In summary, the submarine cable sealant of the present application not only performs well in cross-linking speed and curing efficiency, but also achieves rapid cross-linking at room temperature through the joint action of component A and component B, simplifies the cable production and subsequent sealing construction process, and improves production and construction efficiency. In addition, through the carefully designed component ratio, it effectively improves the comprehensive performance of the sealant, ensures its long-term stability and reliability in complex marine environments, and provides strong technical support for the safe operation of marine communications and power transmission systems.

[0009] Optionally, the A component further comprises the following raw materials in parts by weight: Thickener 8-15 parts; Flame retardant 20-30 parts.

[0010] Optionally, the thickener is selected from hydroxyethyl cellulose; and the flame retardant is selected from modified magnesium hydroxide.

[0011] By adopting the above technical solution, the amount of thickener added can adjust the extrusion test of the material to ensure that the sealant has a suitable viscosity under different production and construction application environments, and is neither too thin to maintain its shape nor too thick to affect construction efficiency. This is conducive to the accurate application of materials on complex structures, while ensuring the morphological stability of the sealant before curing, and reducing sagging and collapse during construction. The modified magnesium hydroxide not only enhances the flame retardant properties of the sealant, but also enhances its interfacial compatibility with the silicone resin due to its surface modification. This modification allows the magnesium hydroxide particles to be more closely combined with the resin network to form a more stable composite structure, thereby improving the overall mechanical strength and thermal stability of the material. Under high temperature conditions, the decomposition products of the modified magnesium hydroxide can also play a role in heat insulation and oxygen isolation, further enhancing the fire resistance of the material.

[0012] Optionally, the dispersant is selected from dipropylene glycol methyl ether.

[0013] By adopting the above technical solution, dipropylene glycol methyl ether as a dispersant plays a vital role in the material preparation process. It can promote the uniform dispersion of each component and ensure the uniformity and stability of the material. In addition, the solvent properties of dipropylene glycol methyl ether help to reduce the viscosity of the material, making the sealant easier to flow and apply during construction, improving construction efficiency and quality.

[0014] Optionally, the method for preparing the acrylated allyl silicone resin comprises the following steps: Step 1: Equivalent amounts of allyl alcohol and acrylic acid are esterified to generate allyl acrylate prepolymer monomer; Step 2: Add the prepared allyl acrylate monomer dropwise into 202 hydrogen-containing silicone oil containing chloroplatinic acid, and stir for 6-10 hours to obtain acrylated allyl silicone resin.

[0015] By adopting the above technical scheme, the preparation method of acrylated allyl silicone resin realizes an efficient and controllable synthesis process through two main steps. First, in step 1, an esterification reaction is carried out by an equivalent amount of allyl alcohol and acrylic acid to generate an allyl acrylate prepolymer monomer. This step solves the problem of low raw material utilization in the traditional synthesis method and ensures the purity of the product and the controllability of the reaction. Then, in step 2, the prepared allyl acrylate monomer is added dropwise to 202 hydrogen-containing silicone oil containing chloroplatinic acid catalyst, and after 6 to 10 hours of stirring reaction, the target product, acrylated allyl silicone resin, is successfully prepared. This method uses chloroplatinic acid as a catalyst to promote the addition reaction between allyl and hydrogen-containing silicone oil, effectively improves the reaction efficiency and shortens the production cycle. In addition, the introduction of acrylated allyl silicone resin not only enhances the adhesion and mechanical strength of the sealant, but also improves the crosslinking efficiency and weather resistance of the sealant through its unique chemical properties, ensuring the long-term performance stability of the sealant in a complex marine environment. Acrylated allyl silicone resin combines the flexibility of silicone with the hardness of acrylate, significantly improving the adhesive properties and mechanical strength of the sealant. This composite structure allows the sealant to maintain good adhesion and recovery when subjected to external impact and deformation, and is not prone to breakage or peeling. The presence of allyl functional groups provides additional cross-linking points for the sealant, forming a denser three-dimensional network structure through free radical polymerization or heat-induced cross-linking reactions. This structure enhances the cohesion of the material. At the same time, the introduction of acrylate segments improves the material's resistance to moisture and other environmental factors, extending the service life of the sealant, especially in harsh marine environments. The sealant prepared by the above technical solution, due to the optimization of its chemical structure and the strengthening of the cross-linking network, can maintain its original physical and chemical properties under long-term exposure to complex marine environmental conditions such as seawater, salt spray, and ultraviolet radiation, prevent aging and degradation, and ensure the long-term stability of the sealing performance of facilities such as ships and offshore platforms. The rheological properties of acrylated allyl silicone resin make the sealant have suitable viscosity and thixotropy during construction, which is easy to apply and shape. At the same time, it shows a low shrinkage rate during the curing process, avoiding stress concentration and cracks, and improving construction efficiency and quality. In summary, the acrylated allyl silicone resin prepared by the above technical solution not only significantly improves the comprehensive performance of the sealant, but also ensures its long-term stability and reliability in complex marine environments. It is suitable for shipbuilding, marine engineering, offshore wind power and other fields, and meets the industry's demand for high-performance sealing materials.

[0016] Optionally, the stirring speed in step 2 is 500-800 r / min.

[0017] Optionally, the vinyl content in the methylphenylvinyl silicone resin is 2-5%.

[0018] By adopting the above technical scheme, the optimization of the vinyl content in methylphenyl vinyl silicone resin realizes the rapid cross-linking of the sealant. At the same time, the flexibility and elasticity of the material are guaranteed, so that it can adapt to the deformation of the submarine cable in the complex terrain of the seabed, effectively prevent seawater penetration, and improve the overall watertight performance. The vinyl functional group in methylphenyl vinyl silicone resin is a key participant in the cross-linking reaction. When the vinyl content is in the range of 2-5%, it can cooperate efficiently with the catalyst in component B (such as butyltin catalyst) to accelerate the cross-linking reaction. This content range ensures sufficient active sites to form a stable and evenly distributed cross-linked network, without being too high to cause excessive cross-linking, affecting the flexibility and processability of the material. The appropriate vinyl content helps to form a moderately cross-linked network structure, which not only ensures the high mechanical strength and toughness of the material, but also maintains good elastic recovery. Too high a vinyl content may cause the cross-linked network to be too dense, making the material brittle and hard, which is not conducive to withstanding the various stresses and deformations that the submarine cable may encounter in a complex marine environment; on the contrary, too low a content may weaken the strength of the cross-linked network and affect the long-term stability and durability of the material. A moderate cross-linked network structure can not only enhance the mechanical properties of the material, but also improve its water tightness and chemical resistance. By controlling the content of vinyl in methylphenyl vinyl silicone resin, the porosity and connectivity of the cross-linked network can be ensured to be in an ideal state, effectively blocking seawater penetration, while reducing the erosion of the material structure by chemicals, which is crucial for the long-term performance of submarine cable sealants in deep-sea environments. In summary, by controlling the content of vinyl in methylphenyl vinyl silicone resin within the range of 2-5%, the submarine cable sealant of this application not only achieves a rapid and uniform cross-linking reaction, but also ensures the high water tightness, chemical stability and mechanical strength of the material in a complex marine environment, providing comprehensive and lasting protection for the safe operation of the submarine cable system. This technical solution fully reflects the ingenuity of the formula design and provides an important reference for the development of high-watertightness room-temperature cross-linkable submarine cable sealants.

[0019] Optionally, the vinyl content in the methylphenylvinyl silicone resin is 4.5%.

[0020] By adopting the above technical solution, the vinyl content in methylphenyl vinyl silicone resin is set to 4.5%, achieving the optimal balance between cross-linking efficiency and material performance, which not only ensures the rapid curing of the sealant, but also maintains its excellent physical and chemical properties, further enhancing the watertightness and durability of the submarine cable sealant.

[0021] Optionally, in the component A, the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin is (1.8-2.3):1.

[0022] By adopting the above technical scheme, by precisely controlling the weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin, the synergistic effect between the internal components of the sealant is achieved, the mechanical properties and chemical stability of the material are enhanced, and the comprehensive performance of the sealant is improved, especially in terms of water tightness and environmental aging resistance. In this application, the weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin is set to (1.8-2.3): 1. The selection of this specific ratio is intended to maximize the comprehensive performance of the sealant by finely regulating the chemical reaction and physical properties between the two key components. Methylphenyl vinyl silicone resin and acrylated allyl silicone resin are key components in component A, and the ratio between them directly affects the formation of the cross-linked network. At a weight ratio of (1.8-2.3): 1, the two resins can work more effectively together to form a denser and more uniform cross-linked network. Such a network structure not only enhances the mechanical strength of the material, but also improves its water tightness and corrosion resistance, ensuring the long-term stable operation of the submarine cable in the deep sea environment. In addition, by precisely controlling the ratio of the two resins, the hardness, elasticity, adhesion and processing properties of the material can be balanced. Excessive amounts of methylphenyl vinyl silicone resin may make the material too hard, affecting its adaptability and sealing effect on complex shapes. The reason may be that methylphenyl vinyl silicone resin contains more phenyl and vinyl groups, which form more crosslinking points in the crosslinking reaction, resulting in an increase in the crosslinking density of the material. Too high a crosslinking density will make the material harder and reduce the free movement space of the molecular chain, thereby reducing the elasticity of the material, making it less adaptable to complex shapes and prone to cracks or breaks, especially at low temperatures or under stress. Excessive amounts of acrylated allyl silicone resin may make the material too soft and reduce its wear and tear resistance. The reason may be that the acrylate groups in acrylated allyl silicone resin have a certain degree of flexibility, and excessive amounts of this resin will lead to an increase in the number of flexible segments in the crosslinked network, making the material as a whole too soft. Although this may improve the ductility and fit of the material, it will also reduce its wear and tear resistance because the material is more likely to deform and be damaged when subjected to friction or impact. In addition, excessive acrylated allyl silicone resin may result in an insufficiently dense cross-linked network, affecting the chemical stability and durability of the material. Especially in deep-sea environments, the material may be more susceptible to corrosion by seawater, salt, and microorganisms, reducing its long-term water tightness and mechanical strength. Therefore, in order to obtain a submarine cable sealant that has both good mechanical strength and wear resistance and sufficient flexibility and processing performance, the ratio between methylphenyl vinyl silicone resin and acrylated allyl silicone resin must be precisely controlled. The specific ratio of the two resins is conducive to the full play of the catalytic effect.At this ratio, the butyl tin catalyst can more efficiently promote the cross-linking reaction between the vinyl in the methylphenyl vinyl silicone resin and the C=C bond in the acrylate in the acrylated allyl silicone resin, accelerate the curing process, and ensure the uniformity and controllability of the cross-linking reaction, avoiding local over- or under-reaction, and improving the stability and consistency of the material. In summary, by setting the weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin to (1.8-2.3): 1, the submarine cable sealant of the present application not only achieves the optimization of the cross-linked network structure, but also ensures the high performance of the material in a complex marine environment, providing comprehensive and lasting protection for the safe operation of the submarine cable system. This technical solution fully reflects the scientific nature and practicality of the formula design, and provides important guidance for improving the performance of high-watertightness room-temperature cross-linkable submarine cable sealants.

[0023] Optionally, the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin is 2:1.

[0024] By adopting the above technical solution, the weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin is set to 2:1. The sealant at this ratio not only has the characteristics of rapid cross-linking, but also exhibits excellent mechanical strength and elastic recovery ability. It can effectively cope with various challenges of submarine cables in harsh environments and ensure the safe operation of the submarine cable system.

[0025] Optionally, in the component A, the weight ratio of the fumed silica to the water-absorbing resin is 1:(4.7-5.3).

[0026] By adopting the above technical solution, the weight ratio of fumed silica and water-absorbing resin is optimized, which significantly enhances the thixotropy and filling properties of the sealant. At the same time, the expansion of the water-absorbing resin when it comes into contact with water further enhances the watertightness of the sealant, effectively preventing the intrusion of seawater and ensuring the long-term reliable operation of the submarine cable system. The weight ratio of the fumed silica and the water-absorbing resin is set to 1: (4.7-5.3). This specific ratio is chosen to achieve the best balance between the mechanical strength, watertightness and processing properties of the material, ensuring the long-term stability and reliability of the submarine cable sealant in a complex marine environment. As a high-performance inorganic filler, fumed silica can significantly improve the mechanical strength and wear resistance of the material. The water-absorbing resin is mainly used to enhance the watertightness of the material. At a weight ratio of 1:(4.7-5.3), fumed silica can effectively fill the voids in the microstructure of the material to form a stable skeleton structure. At the same time, the water-absorbent resin expands after absorbing water, further blocking the tiny voids that are not fully filled. The two work together to significantly improve the mechanical strength and water tightness of the material, ensuring the safety of the submarine cable in the deep sea environment. The water-absorbent resin will quickly absorb water and swell when it comes into contact with water, effectively preventing seawater from penetrating, improving the water tightness and corrosion resistance of the material. The right amount of fumed silica, through its high surface area and good dispersibility, enhances the thixotropy and filling effect of the material, further improving the water tightness. At the above weight ratio, the two components complement each other and jointly construct a multi-layer protective barrier of the material, ensuring the long-term and stable operation of the submarine cable in a complex marine environment. The present application can optimize the processing performance and construction convenience of the material by controlling the weight ratio of fumed silica and water-absorbent resin. Excessive water-absorbing resin may make the material too viscous, affecting the extrusion test and spreadability during construction; while too much fumed silica may increase the hardness of the material and reduce its ductility. At a weight ratio of 1: (4.7-5.3), the material can maintain good extrusion test while having sufficient filling and water tightness, ensuring construction efficiency and sealing effect. Precise weight ratio control not only optimizes the mechanical properties and water tightness of the material, but also ensures the chemical stability and durability of the material in the deep sea environment.

[0027] In summary, by setting the weight ratio of fumed silica to water-absorbing resin to 1:(4.7-5.3), the submarine cable sealant of the present application not only optimizes the material properties, but also ensures its high performance in complex marine environments, providing comprehensive and lasting protection for the safe operation of the submarine cable system. This technical solution fully reflects the scientificity and practicality of the formula design, and provides important guidance for the performance improvement of high watertightness room temperature cross-linkable submarine cable sealants.

[0028] Optionally, the fineness of the water-absorbing resin is not less than 150 meshes.

[0029] By adopting the above technical solution, the fineness of the water-absorbing resin is controlled, which ensures its uniform dispersion in the sealant and avoids local aggregation, thereby improving the overall uniformity and watertightness of the sealant, while also enhancing the processability and construction convenience of the material.

[0030] In a second aspect, the present application provides a method for preparing a high-watertightness room-temperature cross-linkable submarine cable sealant, the preparation method comprising the following steps: The preparation method of the A component comprises the following steps: The preparation method of the A component comprises the following steps: A1. Add polymethylsiloxane, hydroxysiloxane rubber, acrylated allyl silicone resin, methylphenyl vinyl silicone resin and dispersant into a reaction kettle, and stir at 25-30° C. and 300-400 rpm for 10-15 min to obtain a mixture; A2, adding the remaining ingredients in component A to the mixture, increasing the stirring speed to 500-800 rpm, stirring for 15-20 min, cooling, vacuum degassing the obtained mixed liquid, filling it into a plastic finished product bottle, and sealing it with nitrogen to obtain the component A; The preparation method of the B component comprises the following steps: B1. Add butyltin catalyst to polymethylsiloxane and stir at 500-600 rpm for 5-10 min at 25-30°C; B2. Add antioxidant and fumed silica, and stir at 500-600 rpm for 10-15 min at 25-30°C; B3, add 3-glycidyloxypropyl triethoxy silicone oil, stir at 300-400 rpm for 5-8 min at 25-30° C., cool, vacuum degas the obtained mixed liquid, fill it into a plastic finished product bottle, fill it with nitrogen and seal it to obtain the paste B component; Before use and filling, component A and component B are mixed evenly in a mass ratio of 4:(1-4), injected into a mold, and the mold is closed. After 12-48 hours, the mold is opened to obtain the highly watertight room temperature cross-linkable submarine cable sealing rubber elastomer.

[0031] By adopting the above technical scheme, the preparation method proposed in this application ensures uniform mixing and sufficient reaction between the components by strictly controlling the order of addition of raw materials, stirring speed, stirring time and temperature, avoiding the problem of excessive or insufficient local reaction, thereby improving the uniformity and cross-linking efficiency of the sealant. In the preparation process of component A and component B, different stirring conditions are respectively adopted to adapt to the physical and chemical properties of different components, ensuring that each raw material can play a role in the best state. In addition, the steps of vacuum degassing and nitrogen sealing effectively remove the bubbles in the material, improve the density and stability of the sealant, and at the same time, the protective effect of nitrogen avoids the material from being affected by oxygen and moisture during storage and use, ensuring that the long-term performance of the sealant is not damaged. The refined control of the entire preparation process not only ensures the high-quality output of the sealant, but also simplifies the production process, reduces energy consumption, and enhances the market competitiveness of the product.

[0032] In a third aspect, the present application provides an application of a highly watertight submarine cable sealant that can be cross-linked at room temperature in the preparation of submarine cable seals.

[0033] By adopting the above technical solution, the application of the high-watertightness room-temperature cross-linkable submarine cable sealant of the present application in submarine cables has completely revolutionized the sealing technology of submarine cables and high-watertightness cables. Compared with traditional sealants, the sealant of the present application not only has excellent watertightness and chemical stability, can effectively resist seawater erosion, prevent seawater penetration, and ensure the electrical performance and mechanical strength of the submarine cable system, but also its room-temperature cross-linking characteristics greatly simplify the filling process, reduce the requirements for the filling environment, and improve production efficiency. In addition, the long-term stability and durability of the sealant significantly reduce the maintenance frequency and cost of the submarine cable system, provide strong support for the long-term safe operation of the submarine cable system, and are suitable for various complex marine environments. It provides advanced material solutions for the construction and development of global marine communications and power transmission networks.

[0034] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The submarine cable sealant of the present application is specially designed to cope with the extreme environment of the deep sea. It adopts an innovative two-component system. Through the precise proportion and synergistic effect of component A (containing polymethylsiloxane, hydroxysiloxane rubber, methylphenyl vinyl silicone resin, acrylated allyl silicone resin, etc.) and component B (containing polymethylsiloxane, butyl tin catalyst, antioxidant and 3-glycidyl ether oxypropyl triethoxy silicone oil), a cross-linking reaction is initiated at room temperature to form a highly stable three-dimensional network structure. The construction of this network is mainly achieved through the following key chemical reactions: the hydroxyl (-OH) in the hydroxysiloxane rubber and the active groups in other components, under the catalysis of butyl tin catalyst, form Si-O-Si bonds through condensation reaction, construct the basic skeleton of the cross-linked network, and enhance the adhesion and weather resistance of the material. The vinyl group of the methylphenyl vinyl silicone resin and the allyl functional group of the acrylated allyl silicone resin, under the promotion of the catalyst, form CC bonds through free radical polymerization reaction, further enhancing the stability and mechanical strength of the cross-linked network. The ethoxy group in 3-glycidyloxypropyl triethoxy silicone oil reacts with the hydroxyl group of hydroxysiloxane rubber to form an ether bond, which not only strengthens the cross-linking network, but also provides lubrication properties and optimizes the filling properties of the material. The formation of these chemical bonds (Si-O-Si, CC and ether bonds) constructs a complex three-dimensional network densely connected by cross-linking points, which not only gives the material excellent mechanical strength, elasticity, weather resistance and water tightness, but also ensures the stability and integrity of the material structure under extreme pressures of up to 700 atmospheres (equivalent to 700 meters deep sea water pressure), effectively preventing seawater penetration. The sealant simplifies the production process and improves production efficiency. It is particularly suitable for submarine cables and cables with high water tightness requirements. It provides a strong technical guarantee for the safe operation of marine communications and power transmission systems, and represents a major breakthrough in the field of marine engineering technology.

[0035] 2. By setting the weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin to (1.8-2.3):1, the submarine cable sealant of the present application not only achieves the optimization of the cross-linked network structure, but also ensures the high performance of the material in a complex marine environment, providing comprehensive and lasting protection for the safe operation of the submarine cable system. This technical solution fully reflects the scientificity and practicality of the formula design, and provides important guidance for the performance improvement of high watertightness room temperature cross-linkable submarine cable sealants.

[0036] 3. By setting the weight ratio of fumed silica to water-absorbing resin to 1:(4.7-5.3), the submarine cable sealant of the present application not only optimizes the material properties, but also ensures its high performance in complex marine environments, providing comprehensive and lasting protection for the safe operation of the submarine cable system. This technical solution fully reflects the scientificity and practicality of the formula design, and provides important guidance for the performance improvement of high-watertightness room-temperature cross-linkable submarine cable sealants.

[0037] 4. The preparation method proposed in this application ensures uniform mixing and sufficient reaction between the components by strictly controlling the order of adding raw materials, stirring speed, stirring time and temperature, avoiding the problem of excessive or insufficient local reaction, thereby improving the uniformity and cross-linking efficiency of the sealant. The refined control of the entire preparation process not only ensures the high-quality output of the sealant, but also simplifies the production process, reduces energy consumption, and improves the market competitiveness of the product.

[0038] 5. The application of the highly watertight submarine cable sealant that can be cross-linked at room temperature in the submarine cable system of the present application has completely revolutionized the sealing technology of submarine cables, submarine cable joints, and terminals. Compared with traditional sealants, the sealant of the present application not only has excellent watertightness and chemical stability, can effectively resist seawater erosion, prevent seawater infiltration, and ensure the electrical performance and mechanical strength of the submarine cable system, but also its room temperature cross-linking characteristics greatly simplify the submarine cable sealing and filling process, reduce the requirements for the joint and terminal sealing and filling construction environment, improve work efficiency, shorten the installation and maintenance time of submarine cables, and reduce interference with marine ecology. In addition, the long-term stability and durability of the sealant significantly reduce the maintenance frequency and cost of the submarine cable system, provide strong support for the long-term safe operation of the submarine cable system, and are suitable for various complex marine environments. It provides advanced material solutions for the construction and development of global marine communications and power transmission networks. DETAILED DESCRIPTION

[0039] The present application is further described in detail below in conjunction with embodiments. Specific embodiments

[0040] Preparation Example The present invention provides a method for preparing an acrylated allyl silicone resin.

[0041] Preparation Example This preparation example provides an acrylated allyl silicone resin, and the preparation method is as follows: Step 1: 58.06 g of allyl alcohol and 72.06 g of acrylic acid were mixed for esterification reaction to generate allyl acrylate prepolymer monomer; Step 2: Add the prepared allyl acrylate prepolymer monomer to 100 g of 202 hydrogenated silicone oil containing 0.5 g of chloroplatinic acid at a rate of 1 mL / min. The addition process lasts for 30 minutes. After the addition is completed, continue stirring at a rate of 700 r / min for 8 hours; obtain acrylated allyl silicone resin.

[0042] Examples 1-20 provide a highly watertight submarine cable sealant that can be cross-linked at room temperature.

[0043] Example 1 This embodiment provides a highly watertight submarine cable sealant that can be cross-linked at room temperature. The sealant includes component A and component B by weight; component A includes the following raw materials by weight: 120 parts of polymethylsiloxane; 35 parts of hydroxysiloxane rubber; 70 parts of methylphenyl vinyl silicone resin; 35 parts of acrylated allyl silicone resin; 45 parts of dispersant, 4.7 parts of fumed silica; and 25.3 parts of water-absorbing resin.

[0044] The fineness of the water-absorbing resin in this embodiment is 180 mesh.

[0045] The dispersant in this embodiment is dipropylene glycol methyl ether.

[0046] The methylphenylvinyl silicone resin in this embodiment has a vinyl content of 4.5%.

[0047] The acrylated allyl silicone resin in this embodiment is prepared according to the preparation example.

[0048] Component B includes the following raw materials by weight: 30 parts of polymethylsiloxane; 0.3 parts of butyl tin catalyst; 2 parts of fumed silica; 2 parts of antioxidant; 10 parts of 3-glycidyloxypropyl triethoxy silicone oil.

[0049] The preparation method of the high watertight room temperature cross-linkable submarine cable sealant in this embodiment is as follows: The preparation method of component A comprises the following steps: A1. Add polymethylsiloxane, hydroxysiloxane rubber, acrylated allyl silicone resin, methylphenyl vinyl silicone resin and dispersant into a reaction kettle, and stir at 400 rpm for 15 min at 30° C. to obtain a mixture; A2. Add the remaining ingredients in component A to the mixture, increase the stirring speed to 700 rpm, stir for 20 min, cool down, vacuum degas the obtained mixed liquid, fill it into a plastic finished bottle, fill it with nitrogen and seal it to obtain component A; The preparation method of component B comprises the following steps: B1. Add butyltin catalyst to polymethylsiloxane and stir at 600 rpm for 10 min at 30°C; B2. Add antioxidant and fumed silica, and stir at 30°C and 600 rpm for 15 min. B3. Add 3-glycidyloxypropyl triethoxy silicone oil, stir at 400 rpm for 8 minutes at 30°C, cool down, and degas the obtained mixed liquid in vacuum, then fill it into a plastic finished product bottle, fill it with nitrogen and seal it to obtain a paste-like component B; before filling, mix component A and component B in a mass ratio of 4:3, inject them into the mold, close the mold, and open the mold after 24 hours to obtain the highly watertight room temperature cross-linkable submarine cable sealing rubber elastomer.

[0050] Example 2 The difference between this embodiment and embodiment 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 1.8%.

[0051] Example 3 The difference between this embodiment and embodiment 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 2%.

[0052] Example 4 The difference between this embodiment and embodiment 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 4%.

[0053] Example 5 The difference between this embodiment and embodiment 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 5%.

[0054] Example 6 The difference between this embodiment and embodiment 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 5.2%.

[0055] Comparative Examples 1-7 Comparative Example 1 The difference between this comparative example and Example 1 is that, in preparing a high watertight room temperature cross-linkable submarine cable sealant, an equal amount of silicone resin modified acrylate is used instead of acrylated allyl silicone resin. The silicone resin modified acrylate in this comparative example is purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., and the solid content is 50±2%.

[0056] Comparative Example 2 The difference between this comparative example and Example 1 is that, in preparing a high watertight room temperature cross-linkable submarine cable sealant, an equal amount of acrylate-modified silicone resin is used instead of acrylated allyl silicone resin. The acrylate-modified silicone resin in this comparative example is purchased from Hubei Longsheng Sihai New Materials Co., Ltd., with a solid content of 50±1.

[0057] Comparative Example 3 The difference between this comparative example and Example 1 is that no acrylated allyl silicone resin is added when preparing the high watertightness room temperature cross-linkable submarine cable sealant.

[0058] Comparative Example 4 The difference between this comparative example and Example 1 is that, in preparing the high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of methylphenyl vinyl silicone resin is used instead of acrylated allyl silicone resin.

[0059] Comparative Example 5 The difference between this comparative example and Example 1 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of acrylated allyl silicone resin is used instead of methylphenyl vinyl silicone resin.

[0060] Comparative Example 6 The difference between this comparative example and Example 1 is that, in preparing the high watertightness room temperature cross-linkable submarine cable sealant, in component A, an equal amount of fumed silica is used to replace the water-absorbing resin.

[0061] Comparative Example 7 The difference between this comparative example and Example 1 is that, in the preparation of the high watertightness room temperature cross-linkable submarine cable sealant, in component A, an equal amount of water-absorbing resin is used to replace fumed silica.

[0062] Experimental testing: The sealants prepared in Examples 1-8 and Comparative Examples 1-5 were tested as follows: 1. Compressive strength test: Use a tester to test.

[0063] 2. Flame retardant performance: tested in accordance with UL-94 standard.

[0064] 3. Water tightness: Tested in accordance with national standards (CB / T18480-2001, test standard value less than or equal to 1000mm).

[0065] 4. Smoke corrosion performance test: (alternately spray artificial seawater salt mist with a concentration of 5 times that of seawater for 1 day and dry for 1 day, totaling 120 days).

[0066] 5. Extrusion test: Extrusion is tested in accordance with GB / T 16776-2005.

[0067] 6. Temperature resistance test: The glass transition temperature is tested using the glass transition temperature tester DSC-100.

[0068] 7. Surface drying time: Surface drying time is tested according to GB / T13477.3-2017.

[0069] The experimental test results of Examples 1-6 and Comparative Examples 1-3 are shown in Table 1.

[0070] Table 1 - Experimental test results of Examples 1-6 and Comparative Examples 1-7 Result analysis: The difference between Example 2-6 and Example 1 is that when preparing high watertightness and room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is different. Combined with the experimental test data in Table 1, it can be seen that when the content of vinyl is about 4.5% when preparing methylphenyl vinyl silicone resin, the comprehensive performance of the obtained sealant is better.

[0071] The difference between Example 2 and Example 1 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 1.8%. The difference between Example 6 and Example 1 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the content of vinyl in the methylphenyl vinyl silicone resin is 5.2%. Combining the experimental data of Example 1, Example 2 and Example 6, it can be seen that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, too much or too little vinyl in the methylphenyl vinyl silicone resin will affect the compressive strength of the sealant. The reason may be that the vinyl content directly affects the cross-linking density and distribution inside the material. An appropriate amount of vinyl can effectively enhance the cross-linking network through free radical polymerization, which not only ensures sufficient mechanical strength, but also maintains good elasticity and sealing. Improper content may cause insufficient or excessive cross-linking, affecting the physical properties of the material.

[0072] The difference between Comparative Example 1 and Example 1 is that, when preparing a high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of silicone resin modified acrylate is used instead of acrylated allyl silicone resin. Combining the experimental test data of Example 1 and Comparative Example 1, it can be seen that the replacement of acrylated allyl silicone resin with silicone resin modified acrylate will lead to a decrease in the compressive strength and watertightness of the prepared sealant. The reason may be that the special structure in acrylated allyl silicone resin is essential for forming a stable cross-linked network and improving watertightness. The silicone resin modified acrylate may not be able to participate in the cross-linking reaction as effectively as the original component, or its cross-linking structure is not as tight as the original component, thereby affecting the overall performance.

[0073] The difference between Comparative Example 2 and Example 1 is that, in preparing a high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of silicone resin is used instead of acrylated allyl silicone resin. Combining the experimental test data in Table 1, it can be seen that if silicone resin is used instead of acrylated allyl silicone resin, the compressive strength, watertightness and smoke corrosion are all reduced. The reason may be that acrylated allyl silicone resin plays an irreplaceable role in providing specific functional groups to promote cross-linking, enhance water molecule repellency and improve chemical stability.

[0074] The difference between Comparative Example 3 and Example 1 is that no acrylated allyl silicone resin was added when preparing the high watertightness room temperature cross-linkable submarine cable sealant. Combined with the experimental test data in Table 1, it can be seen that if acrylated allyl silicone resin is not used at all when preparing the sealant, the compressive strength and watertightness will be significantly reduced, which once again proves the cornerstone role of this component in the performance of the sealant, and its absence directly affects the cross-linking efficiency and water molecule barrier performance of the material.

[0075] The difference between Comparative Example 4 and Example 1 is that, in preparing the high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of methylphenyl vinyl silicone resin is used instead of acrylated allyl silicone resin.

[0076] The difference between Comparative Example 5 and Example 1 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, an equal amount of acrylated allyl silicone resin is used instead of methylphenyl vinyl silicone resin. Combined with the experimental data in Table 1, it can be seen that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the watertightness and compressive strength of the sealant can be improved when methylphenyl vinyl silicone resin and acrylated allyl silicone resin are compounded. The reason may be that the vinyl in methylphenyl vinyl silicone resin can form CC cross-linking bonds through free radical polymerization, providing good mechanical strength and heat resistance; while the allyl functional group in the acrylated allyl silicone resin not only participates in cross-linking itself, but also reacts with the hydroxyl group in the hydroxyl silicone rubber to form COC cross-linking bonds, thereby enhancing the diversity and stability of the network. This diversified cross-linking structure improves the overall toughness and compressive strength of the material. In addition, different polymer segments can form a denser intermolecular arrangement by blending, which is conducive to reducing the formation of micropores, thereby improving watertightness. The different polarities and functional groups of methylphenyl vinyl silicone resin and acrylated allyl silicone resin interact with each other, which may promote tighter molecular stacking and enhance the sealing effect. By adjusting the ratio of the two, the relationship between hardness and elasticity, adhesion and durability can be balanced. Methylphenyl vinyl silicone resin tends to provide better rigidity and chemical resistance, while acrylated allyl silicone resin enhances the flexibility and adhesion of the material. At a specific ratio, this balance is optimal, making the sealant not easily damaged by external forces, but also able to adapt well to substrate deformation and maintain long-term sealing performance. Therefore, by finely adjusting the ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin, the best synergy between the two can be achieved, which not only improves the watertightness and compressive strength of the sealant, but also may optimize its processing performance and long-term stability, which is particularly important for meeting the harsh use environment of deep-sea cables.

[0077] The difference between Comparative Example 6 and Example 1 is that when preparing a highly watertight room temperature cross-linkable submarine cable sealant, an equal amount of fumed silica is used instead of a water-absorbing resin. Combined with the experimental test data in Table 1, it can be seen that when preparing a sealant, replacing the water-absorbing resin with fumed silica will result in a decrease in the water tightness of the sealant. The reason may be that in Comparative Example 6, the water-absorbing resin is completely replaced by fumed silica. Although the use of fumed silica on the basis of Example 1 can improve the compressive strength of the sealant to a certain extent, too much fumed silica will affect the overall extrusion test of the sealant, and may also affect the curing process and water tightness of the sealant. The reason may be that excessive addition of fumed silica may affect the curing process of the sealant. Due to its high dispersibility, excessive fumed silica may interfere with the cross-linking reaction, resulting in a slowed curing rate or incomplete curing, thereby affecting the final mechanical strength and elasticity. Excessive addition of fumed silica can significantly increase the viscosity of the sealant, which may reduce its extrusion test, making it difficult for the sealant to fully fill all the details that need to be sealed during construction, thereby affecting the overall water tightness. The network structure formed by fumed silica may be too dense, affecting the elasticity of the sealant, resulting in the sealant may not be able to effectively restore its original state when subjected to external stress, forming tiny cracks, and then affecting water tightness. Excessive addition of fumed silica may affect the interfacial adhesion between the sealant and the substrate. If the sealant and the substrate fail to form a strong adhesion, water molecules may penetrate from these weak interfaces and reduce water tightness. Although fumed silica itself has an extremely high specific surface area, which helps to form a dense structure, excessive addition may also lead to uneven internal porosity and form micropores that are not conducive to water tightness. In addition, fumed silica is a relatively expensive material, and excessive addition will directly increase the production cost of the sealant, which is especially important in large-scale production. In addition, fumed silica is a paste, and if a large amount is added, it will lead to poor extrusion test.

[0078] The difference between Comparative Example 7 and Example 1 is that an equal amount of water-absorbing resin is used to replace fumed silica when preparing a high water-tightness room temperature cross-linkable submarine cable sealant. Combined with the experimental test data in Table 3, it can be seen that when an equal amount of water-absorbing resin is used to replace fumed silica when preparing a high water-tightness room temperature cross-linkable submarine cable sealant, the compressive strength and water-tightness of the prepared sealant are both poor. The reason may be that the compressive strength and water-tightness are both poor when the same amount of water-absorbing resin is used to completely replace fumed silica. Although the water-tightness should be improved in theory, due to the lack of mechanical support and thickening effect provided by fumed silica, the structural stability of the sealant is greatly reduced, and the compressive strength is weakened. At the same time, too much water-absorbing resin may cause the material to be too soft and unable to withstand the deep-sea high-pressure environment, which indirectly affects the water-tightness.

[0079] In summary, the reasonable ratio of fumed silica and water-absorbing resin in sealant is crucial to achieving good comprehensive performance. Both are indispensable and need to be precisely adjusted to achieve the best performance balance.

[0080] Example 7 The difference between this embodiment and embodiment 1 is that the component A in this embodiment further includes 8 parts of a thickener, which is selected from hydroxyethyl cellulose; 20 parts of a flame retardant, which is selected from magnesium hydroxide prepared by a chemical method (commercially available from Guangdong Yongfeng Chemical Co., Ltd., product specification YF01); Component B includes the following raw materials by weight: 30 parts of polymethylsiloxane; 0.3 parts of butyl tin catalyst; 2 parts of antioxidant; 3-glycidyloxypropyl triethoxy silicone oil (commercially available, provided by Nanjing Nengde New Materials), 2 parts of fumed silica.

[0081] The preparation method of the high watertight room temperature cross-linkable submarine cable sealant in this embodiment is as follows: The preparation method of component A comprises the following steps: A1. Add polymethylsiloxane, hydroxysiloxane rubber, acrylated allyl silicone resin, methylphenyl vinyl silicone resin and dispersant into a reaction kettle, and stir at 400 rpm for 15 min at 30° C. to obtain a mixture; A2. Add the remaining ingredients in component A to the mixture, increase the stirring speed to 700 rpm, stir for 20 min, cool down, vacuum degas the obtained mixed liquid, fill it into a plastic finished bottle, fill it with nitrogen and seal it to obtain component A; The preparation method of component B comprises the following steps: B1. Add butyltin catalyst to polymethylsiloxane and stir at 600 rpm for 10 min at 30°C; B2. Add antioxidant and fumed silica, and stir at 30°C and 600 rpm for 15 min. The experimental test results of Example 7 are shown in Table 2.

[0082] Table 2-Experimental test results of the embodiment Result analysis: The difference between Example 8 and Example 7 is that when preparing a high watertight room temperature cross-linkable submarine cable sealant, component A also includes a thickener (hydroxyethyl cellulose), a flame retardant (modified magnesium hydroxide), and a lubricant (3-glycidyloxypropyl triethoxy silicone oil). Combined with the experimental test results in Table 2, it can be seen that adding a thickener, modified magnesium hydroxide, and 3-glycidyloxypropyl triethoxy silicone oil to Example 7 can not only improve the flame retardancy, but also improve the compressive strength, watertightness, and smoke corrosion performance of the obtained sealant to a certain extent.

[0083] Embodiment 8-10 The difference between Examples 8-10 and Example 7 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the total weight of the methylphenyl vinyl silicone resin and the acrylated allyl silicone resin remains unchanged, and the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin changes.

[0084] Example 8 The difference between this embodiment and embodiment 7 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the total weight of methylphenyl vinyl silicone resin and acrylated allyl silicone resin is 105 parts, and the weight ratio of methylphenyl vinyl silicone resin to acrylated allyl silicone resin is 1.8:1.

[0085] Example 9 The difference between this embodiment and embodiment 7 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the total weight of methylphenyl vinyl silicone resin and acrylated allyl silicone resin is 105 parts, and the weight ratio of methylphenyl vinyl silicone resin to acrylated allyl silicone resin is 2.2:1.

[0086] Example 10 The difference between this embodiment and embodiment 7 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, the total weight of methylphenyl vinyl silicone resin and acrylated allyl silicone resin is 105 parts, and the weight ratio of methylphenyl vinyl silicone resin to acrylated allyl silicone resin is 2.3:1.

[0087] The experimental test results of Examples 8-10 are shown in Table 3.

[0088] Table 3 - Experimental test results of Examples 8-10 Result analysis: The difference between Examples 8-10 and Example 7 is that, when preparing a high watertight room temperature cross-linkable submarine cable sealant, the total weight of the methylphenyl vinyl silicone resin and the acrylated allyl silicone resin remains unchanged, and the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin changes. Combined with the experimental test data in Table 3, it can be seen that when the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin is 2:1, the comprehensive performance of the obtained sealant is better.

[0089] Examples 11-13 The difference between Examples 11-13 and Example 7 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the total weight of the fumed silica and the water-absorbing resin is 30 parts, and the weight ratio of the fumed silica and the water-absorbing resin is different.

[0090] Embodiment 11 The difference between this embodiment and embodiment 7 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the total weight of the fumed silica and the water-absorbing resin is 30 parts, and the weight ratio of the fumed silica to the water-absorbing resin is 1:4.7.

[0091] Example 12 The difference between this embodiment and embodiment 7 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the total weight of the fumed silica and the water-absorbing resin is 30 parts, and the weight ratio of the fumed silica to the water-absorbing resin is 1:5.

[0092] Example 13 The difference between this embodiment and embodiment 7 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the total weight of the fumed silica and the water-absorbing resin is 30 parts, and the weight ratio of the fumed silica to the water-absorbing resin is 1:5.5.

[0093] Table 4 - Experimental test results of Examples 11-13 and Comparative Examples 8-9 Result analysis: The difference between Examples 11-13 and Example 7 is that when preparing a highly watertight room temperature cross-linkable submarine cable sealant, the total weight of fumed silica and water-absorbing resin is 30 parts, and the weight ratio of fumed silica and water-absorbing resin is different. Combined with the experimental test data in Table 4, it can be seen that when preparing a sealant, the weight ratio of fumed silica to water-absorbing resin is 1:5, which can better improve the comprehensive performance of the prepared sealant. When the weight ratio of fumed silica to water-absorbing resin is 1:5, this ratio can effectively balance the mechanical properties (such as compressive strength) and water-tightness of the sealant. Fumed silica provides the necessary structural support and thickening effect, while the water-absorbing resin strengthens the sealing of tiny gaps through its water absorption and expansion characteristics. The synergistic effect of the two enables the sealant to achieve the best comprehensive performance after cross-linking at room temperature. The uniqueness of the water-absorbing resin lies in its ability to absorb and retain moisture, especially when it encounters water, it can quickly expand to form a gel, block tiny pores, thereby effectively blocking moisture penetration and greatly enhancing the water tightness of the material. This property is crucial for submarine cable sealants, as they need to maintain sealing performance for a long time in a high-pressure water environment. As an important filler, fumed silica's main functions include thickening, improving thixotropy and enhancing mechanical properties. It can form a network structure, effectively preventing the material from flowing when stressed, increasing the structural stability of the sealant, and also improving the compressive strength. In addition, the hydroxyl groups on the surface of fumed silica can participate in the cross-linking reaction, further strengthening the cross-linking network and improving the overall performance of the material.

[0094] Examples 14-15 The difference between Example 14-15 and Example 12 is that when preparing the high watertightness room temperature cross-linkable submarine cable sealant, the weight percentages of some components are changed. The differences are shown in Table 5.

[0095] Table 5 - Differences between Examples 14-15 and Example 12 Ingredients (portions) Example 12 Embodiment 14 Embodiment 15 Polymethylsiloxane 120 138 150 Hydroxysiloxane rubber 35 43 50 Methylphenylvinyl silicone resin 70 70 70 Acrylated Allyl Silicone Resin 35 35 35 Fumed Silica 5 7 8 Water-absorbent resin 25 35 40 Thickener 8 13 15 Dipropylene glycol methyl ether 45 68 75 Modified magnesium hydroxide 20 27 30 3-Glycidyloxypropyl triethoxy silicone oil 20 36 40 Butyltin catalyst 0.3 0.4 0.5 Antioxidants 2 5 6 3-Glycidyloxypropyl triethoxy silicone oil 10 13 15 The experimental test results of Examples 14-15 are shown in Table 6.

[0096] Table 6 - Experimental test results of Examples 14-15 Result analysis: Combined with the experimental test results in Table 6, it can be seen that when preparing a high watertight submarine cable sealant that can be cross-linked at room temperature, the weight proportions of some components are different. Combined with the experimental test results in Table 6, it can be seen that the comprehensive performance of the high watertight submarine cable sealant that can be cross-linked at room temperature prepared by Example 14 is better.

[0097] Examples 16-20 The difference between Examples 16-20 and Example 14 is that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, based on the premise that the weight ratio of methylphenyl vinyl silicone resin to acrylated allyl silicone resin is 2:1, the total weight ratio of methylphenyl vinyl silicone resin and acrylated allyl silicone resin in the high watertightness room temperature cross-linkable submarine cable sealant is changed, and a better weight ratio is selected.

[0098] In Example 16, the total weight of the methylphenyl vinyl silicone resin and the acrylated allyl silicone resin is 105 parts, and the total weight of the high water-tightness room temperature cross-linkable submarine cable sealant is 490.4 parts.

[0099] Therefore, it is not difficult to conclude that in Example 16, the proportion of methylphenyl vinyl silicone resin (referred to as variable 1) and acrylated allyl silicone resin (referred to as variable 2) in the high watertight room temperature cross-linkable submarine cable sealant (referred to as the matrix) is 21.41%.

[0100] The differences between Examples 16-20 and Example 14 are shown in Table 7.

[0101] Proportion = (variable 1 + variable 2) / total weight of matrix * 100%.

[0102] Table 7 - Differences between Examples 16-20 and Example 14 See Table 8 for the experimental test results of Examples 16-20.

[0103] Table 8 - Experimental test results of Examples 16-20 Result analysis: Combined with the experimental test results in Table 8, it can be seen that when preparing a high watertightness room temperature cross-linkable submarine cable sealant, when the total weight of methylphenyl vinyl silicone resin (referred to as variable 1) and acrylated allyl silicone resin (referred to as variable 2) in the high watertightness room temperature cross-linkable submarine cable sealant is 21-24%, the comprehensive performance of the high watertightness room temperature cross-linkable submarine cable sealant is better. When the total weight of methylphenyl vinyl silicone resin (referred to as variable 1) and acrylated allyl silicone resin (referred to as variable 2) in the high watertightness room temperature cross-linkable submarine cable sealant is 23.2%, the comprehensive performance of the high watertightness room temperature cross-linkable submarine cable sealant is the best.

[0104] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A highly watertight room temperature cross-linkable submarine cable sealant, It is characterized in that The sealant comprises component A and component B in parts by weight; The A component includes the following raw materials by weight: 120-150 parts of polymethylsiloxane; 35-50 parts of hydroxy silicone rubber; 60-80 parts of methylphenyl vinyl silicone resin; 30-40 parts of acrylated allyl silicone resin; Dispersant 45-75 parts; 5-10 parts of fumed silica; 25-50 parts of water-absorbing resin; The B component includes the following raw materials by weight: 30-50 parts of polymethylsiloxane; 0.3-0.5 parts of butyl tin catalyst; 2-6 parts of antioxidant; 2-5 parts of fumed silica; 3-glycidyl ether oxypropyl triethoxy silicone oil 10-15 parts.

2. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that The A component also includes the following raw materials in parts by weight: Thickener 8-15 parts; Flame retardant 20-30 parts.

3. A highly watertight room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that The method for preparing the acrylated allyl silicone resin comprises the following steps: Step 1: Equivalent amounts of allyl alcohol and acrylic acid are esterified to generate allyl acrylate prepolymer monomer; Step 2: Add the prepared allyl acrylate prepolymer monomer dropwise into 202 hydrogen-containing silicone oil containing chloroplatinic acid, and stir for 6-10 hours to obtain acrylated allyl silicone resin.

4. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 3, It is characterized in that The stirring speed in step 2 is 500-800 r / min.

5. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that The content of vinyl in the methylphenyl vinyl silicone resin is 2-5%.

6. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that In the component A, the weight ratio of the methylphenyl vinyl silicone resin to the acrylated allyl silicone resin is (1.8-2.3):

1.

7. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that In the component A, the weight ratio of the fumed silica to the water-absorbing resin is 1:(4.7-5.3).

8. The high watertightness room temperature cross-linkable submarine cable sealant according to claim 1, It is characterized in that The fineness of the water-absorbing resin is not less than 150 meshes.

9. A method for preparing the highly watertight room temperature cross-linkable submarine cable sealant according to any one of claims 1 to 8, It is characterized in that The preparation method comprises the following steps: The preparation method of the A component comprises the following steps: A1. Add polymethylsiloxane, hydroxysiloxane rubber, acrylated allyl silicone resin, methylphenyl vinyl silicone resin and dispersant into a reaction kettle, and stir at 25-30° C. and 300-400 rpm for 10-15 min to obtain a mixture; A2, adding the remaining ingredients in component A to the mixture, increasing the stirring speed to 500-800 rpm, stirring for 15-20 min, cooling, vacuum degassing the obtained mixed liquid, filling it into a plastic finished product bottle, and sealing it with nitrogen to obtain the component A; The preparation method of the B component comprises the following steps: B1. Add butyltin catalyst to polymethylsiloxane and stir at 500-600 rpm for 5-10 min at 25-30°C; B2, adding antioxidant and fumed silica, stirring at 500-600 rpm for 10-15 min at 25-30°C; B3, add 3-glycidyloxypropyl triethoxy silicone oil, stir at 300-400 rpm for 5-8 min at 25-30 ° C, cool, and vacuum degas the obtained mixed liquid, fill it into a plastic finished product bottle, and seal it with nitrogen to obtain the paste B component; Before use and filling, component A and component B are mixed evenly in a mass ratio of 4: (1-4), injected into a mold, and the mold is closed. After 12-48 hours, the mold is opened to obtain the highly watertight room temperature cross-linkable submarine cable sealing rubber elastomer.

10. Use of the highly watertight room temperature cross-linkable submarine cable sealant according to any one of claims 1 to 8 in submarine cable sealing.

Citation Information

Patent Citations

  • Novel functional group-containing fluorine-modified silicone oils and preparation method thereof

    CN104086776A

  • Crude oil demulsifier containing organic silicon and preparation method

    CN106479559A

Cited By

  • Organic silicon resin sealant and preparation method thereof

    CN121182451A