Method for preparing synthesis gas by coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification two-step method

By employing a two-step method of lignite dry distillation pyrolysis in a coking furnace followed by coke fixed-bed gasification, high-value utilization of lignite has been achieved, solving the problems of low coking coal prices and lignite pollution, and improving the economic benefits of coking enterprises and the clean utilization efficiency of coal.

CN118931572APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411266423.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the current technology, the price of coking coal is low, coking enterprises suffer serious losses, and lignite, as a low-value fuel, pollutes the air, so there is an urgent need for efficient and clean utilization solutions.

Method used

A two-step method of coking furnace lignite dry distillation pyrolysis and coke fixed-bed gasification is adopted. The process involves grinding lignite and dry distilling and pyrolyzing it in a coking furnace to produce coke oven gas and lignite coke. Then, water gas is produced in a fixed-bed gasifier using steam and oxygen as gasifying agents, thereby realizing the high-value utilization of lignite.

Benefits of technology

It reduces the operating costs of coal coking furnaces, increases the value output of lignite, produces coal gas that can be used in the chemical industry, and enhances the profitability of coking enterprises and the clean and efficient utilization of coal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005037268050000011
    Figure HDA0005037268050000011
Patent Text Reader

Abstract

The invention discloses a method for preparing synthesis gas by a coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification two-step method, which comprises the following steps: levigating lignite, adding into a coking furnace carbonization chamber, tamping, carrying out dry distillation pyrolysis and coking to obtain lignite coke, cooling the lignite coke, feeding into a coal mill, levigating, conveying into a fixed bed gasification furnace, and carrying out fixed bed gasification to obtain the synthesis gas. Introducing water vapor and oxygen as gasifying agents into the gasification furnace from the lower part, and carrying out fixed bed gasification furnace gasification to finally obtain ash and synthesis gas; the low-value lignite is used as a main raw material, high-quality coal gas is obtained through coking furnace production process adjustment and technical transformation, and the method has important significance on cost reduction and efficiency improvement in the coking industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal chemical utilization, and in particular to a method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification. Background Art

[0002] Coal coking is an important way to convert coal into clean energy using coal as raw material, and it plays an important role in coal processing. Coal coking is the process of processing coal into products such as coal gas, tar, and coke through high-temperature dry distillation (900-1000°C) or medium-low temperature dry distillation (500-900°C). Coking coal is a kind of bituminous coal, mainly including lean coal, lean coal, coking coal, fat coal, 1 / 3 coking coal, gas fat coal, gas coal, and 1 / 2 medium sticky coal.

[0003] Coke is the most important product of coking. More than 90% of coke is used for blast furnace ironmaking, followed by foundry and non-ferrous metal smelting industries, and a small amount is used to produce calcium carbide, carbon disulfide, elemental phosphorus, etc. At present, however, with the slowdown in economic growth, the sharp drop in downstream demand, and the "big dive" in steel prices, facing such a severe market situation, steel mills have taken measures to reduce production and limit production, resulting in generally poor coking coal profits, a serious loss per ton of coke nationwide, and a large number of coking plants transforming to survive.

[0004] At present, the coking industry has a strong market for coking byproducts such as methanol, ammonia, and hydrogen peroxide, but due to the impact of the coke market, the company has suffered serious losses and is in urgent need of a "more byproducts and less coke" technical upgrade plan. Lignite is a mineral coal with the lowest degree of coalification, between peat and bituminous coal, with a low carbon content and a low calorific value of 11 to 17 MJ / kg. In addition, it contains more impurities and volatile substances and a high water content. It is often used for combustion in power station boilers. When burned, it will pollute the air. It is mainly used as fuel for power plants, and the price is 300 to 400 yuan / ton. Through the technical transformation of coking furnaces, the use of lignite to replace coking coal to produce coal chemical byproducts is realized, which is of great significance to the coking enterprise to improve the profitability and clean and efficient use of coal. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention relies on traditional coking furnaces to achieve clean and efficient comprehensive utilization of lignite, and produces coal gas, the basic raw material for coal chemical industry. The produced coal gas can be applied to by-product chemical fields such as methanol, ammonia, and hydrogen peroxide, thereby achieving high-value utilization of lignite, promoting cost reduction and efficiency improvement of coking enterprises, and realizing high-value, clean and low-carbon utilization of low-grade coal resources.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification, the specific steps are as follows:

[0008] (1) grind lignite into fine powder and add it into the carbonization chamber of the coking furnace, tamp it and then perform dry distillation and pyrolysis to obtain lignite coke;

[0009] (2) The lignite coke is cooled and sent to a coal mill for grinding and then sent to a fixed bed gasifier. Water vapor and oxygen are used as gasifying agents and introduced into the fixed bed gasifier from the bottom. After gasification in the fixed bed gasifier, ash and synthesis gas are finally obtained.

[0010] Step (1) The lignite particle size is ground to 3-10 mm.

[0011] The temperature of the dry distillation and pyrolysis in step (1) is 600° C. to 1100° C., and the time is 4 to 10 hours.

[0012] Step (2) The lignite coke is ground to a particle size of 0.9 to 5.0 mm.

[0013] The gasification working temperature of the fixed bed gasifier in step (2) is 700°C to 1300°C.

[0014] In step (2), the mass ratio of lignite coke to water vapor during the gasification process in the fixed bed gasifier is 1:0.3 to 1:1.3.

[0015] In step (2), the air-fuel ratio of oxygen to lignite coke in the fixed bed gasifier gasification process is 0.1:1 to 0.4:1.

[0016] The technical effects of the present invention are:

[0017] (1) The method of the present invention is simple. Lignite is used to replace coking coal in a coking furnace for dry distillation and pyrolysis to produce coke oven gas and lignite coke. The lignite coke is then cooled, ground and transported to a fixed bed gasifier. Water gas is produced using water vapor and oxygen as gasifying agents, thereby reducing the operating cost of the coal coking furnace and increasing the value output of lignite. Coke oven gas and water gas are produced respectively. The prepared gas can be used in the chemical industry, thereby achieving clean and efficient utilization of coal.

[0018] (2) The present invention is simple to transform the coking furnace into during its application, and can realize the seamless switching of coking coal and lignite in the same carbonization chamber and the synchronous feeding production in different carbonization chambers, thereby improving the applicability and utilization efficiency of the coking furnace. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The present invention is a flow chart of a method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification. DETAILED DESCRIPTION

[0020] In order to make the technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to the described contents.

[0021] Example 1

[0022] A method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification, such as Figure 1 As shown, the following steps are included:

[0023] (1) Taking lignite with a moisture content of 12.49wt%, an ash content of 3.58wt%, a volatile matter content of 43.72wt%, and a fixed carbon content of 40.21wt% as an example, the lignite is ground to a particle size of 3-10mm, transported to the site by a lignite loading truck to replace coking coal, and then added to the carbonization chamber of the coking furnace. After tamping, it is subjected to dry distillation and pyrolysis at 600°C. After 10 hours, lignite coke is obtained by coking, with a yield of 61.5%. The coke oven gas generated during the dry distillation and pyrolysis process is sent to the bridge pipe through a riser, and then the coke oven gas is collected in the gas collecting pipe. A part of the gas is purified by dry dust removal, and the gas is detected and analyzed by a gas analyzer. The hydrogen content in the coke oven gas is 24.81vol.%, the carbon monoxide content is 37.4vol.%, the carbon dioxide content is 4.02vol.%, and the methane content is 33.77vol.%. The other part of the gas is returned to the return gas main pipe and enters the combustion chamber for combustion;

[0024] (2) using a coke pusher to guide the lignite coke from step (1) into the coke quenching car of the coke blocking car, using dry coke quenching, and sending the cooled lignite coke to a coal mill to grind the particle size to 0.9 to 5.0 mm;

[0025] (3) The ground lignite coke is transported to a fixed-bed gasifier, and a mixture of water vapor and oxygen is introduced into the gasifier from the bottom as a gasifying agent, wherein the mass ratio of lignite coke to water vapor is 1:1.3, and the air-fuel ratio of oxygen to lignite coke is 0.1:1. The gasification temperature of the fixed-bed gasifier is 800°C. After the reaction is complete and the slag is discharged, 6.58% ash is obtained. The furnace gas is collected through a gas collecting pipe, and the gasifier gas is purified by dry dust removal. The gasifier gas is detected and analyzed by a gas analyzer. The hydrogen content in the gasifier gas is 64.34 vol.%, the carbon monoxide content is 25.46 vol.%, and the carbon dioxide content is 10.2 vol.%. No methane and tar are detected.

[0026] Example 2

[0027] A method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification comprises the following steps:

[0028] (1) Taking lignite with a moisture content of 12.49 wt%, an ash content of 3.58 wt%, a volatile matter content of 43.72 wt%, and a fixed carbon content of 40.21 wt% as an example, the lignite is ground to 3-10 mm, transported to the site by a lignite loading truck to replace coking coal, and then added to the carbonization chamber of the coking furnace. After tamping, it is subjected to dry distillation and pyrolysis at 900°C. After 7 hours, lignite coke is obtained by coking, with a yield of 53.1%. The coke oven gas generated during the dry distillation and pyrolysis process is sent to the bridge pipe through a riser, and then the coke oven gas is collected in the gas collecting pipe. A part of the gas is purified by dry dust removal, and the gas is detected and analyzed by a gas analyzer. The hydrogen content in the coke oven gas is 47.81 vol.%, the carbon monoxide content is 36.6 vol.%, the carbon dioxide content is 3.12 vol.%, and the methane content is 12.47 vol.%. The other part of the gas is returned to the return gas main pipe and enters the combustion chamber for combustion;

[0029] (2) using a coke pusher to guide the lignite coke from step (1) into the coke quenching car of the coke blocking car, using dry coke quenching, and sending the cooled lignite coke to a coal mill to grind the particle size to 0.9 to 5.0 mm;

[0030] (3) The ground lignite coke is transported to a fixed-bed gasifier, and a mixture of water vapor and oxygen is introduced into the gasifier from the bottom as a gasifying agent, wherein the mass ratio of lignite coke to water vapor is 1:1, and the air-fuel ratio of oxygen to lignite coke is 0.25:1. The gasification temperature of the fixed-bed gasifier is 1100°C. After the reaction is complete and the slag is discharged, ash of 6.01% is obtained. The furnace gas is collected through a gas collecting pipe, and the gasifier gas is purified by dry dust removal. The gasifier gas is detected and analyzed by a gas analyzer. The hydrogen content in the gasifier gas is 49.48 vol.%, the carbon monoxide content is 30.85 vol.%, and the carbon dioxide content is 19.67 vol.%. No methane and tar are detected.

[0031] Example 3

[0032] A method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification comprises the following steps:

[0033] (1) Taking lignite containing 9.56wt% of moisture, 10.40wt% of ash, 29.20wt% of volatile matter and 50.84wt% of fixed carbon as an example, the lignite is ground to 3-10mm, transported to the site by a lignite loading truck to replace coking coal, and then added to the carbonization chamber of the coking furnace. After tamping, it is subjected to dry distillation and pyrolysis at 700°C. After 8 hours, lignite coke is obtained by coking, with a yield of 64.4%. The coke oven gas generated during the dry distillation and pyrolysis process is sent to the bridge pipe through a riser, and then the coke oven gas is collected in the gas collecting pipe. A part of the gas is purified by dry dust removal, and the gas is detected and analyzed by a gas analyzer. The hydrogen content in the coke oven gas is 43.31vol.%, the carbon monoxide content is 30.9vol.%, the carbon dioxide content is 4.62vol.%, and the methane content is 21.17vol.%. The other part of the gas is returned to the return gas main pipe and enters the combustion chamber for combustion;

[0034] (2) using a coke pusher to guide the lignite coke from step (1) into the quenching car of the coke blocking car, using water cooling to quench the coke, and sending the cooled lignite coke to a coal mill to grind the particle size to 0.9 to 5.0 mm;

[0035] (3) The ground lignite coke is transported to a fixed-bed gasifier, and a mixture of water vapor and oxygen is introduced into the gasifier from the bottom as a gasifying agent, wherein the mass ratio of lignite coke to water vapor is 1:0.5, and the air-fuel ratio of oxygen to lignite coke is 0.3:1. The gasification temperature of the fixed-bed gasifier is 900°C. After the reaction is complete and the slag is discharged, 17.82% ash is obtained. The furnace gas is collected through a gas collecting pipe, and the gasifier gas is purified by dry dust removal. The gasifier gas is detected and analyzed by a gas analyzer. The hydrogen content in the gasifier gas is 42.65 vol.%, the carbon monoxide content is 38.55 vol.%, and the carbon dioxide content is 18.8 vol.%. No methane and tar are detected.

[0036] Example 4

[0037] A method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification comprises the following steps:

[0038] (1) Taking lignite with a moisture content of 9.56 wt%, an ash content of 10.40 wt%, a volatile matter content of 29.20 wt%, and a fixed carbon content of 50.84 wt% as an example, the lignite is ground to 3-10 mm, transported to the site by a lignite loading truck to replace coking coal, and then added to the carbonization chamber of the coking furnace. After tamping, it is subjected to dry distillation and pyrolysis at 800°C. After 9 hours, lignite coke is obtained by coking, with a yield of 60.5%. The coke oven gas generated during the dry distillation and pyrolysis process is sent to the bridge pipe through a riser, and then the coke oven gas is collected in the gas collecting pipe. A part of the gas is purified by dry dust removal, and the gas is detected and analyzed by a gas analyzer. The hydrogen content in the coke oven gas is 50.22 vol.%, the carbon monoxide content is 31.1 vol.%, the carbon dioxide content is 3.83 vol.%, and the methane content is 14.85 vol.%. The other part of the gas is returned to the return gas main pipe and enters the combustion chamber for combustion;

[0039] (2) using a coke pusher to guide the lignite coke from step (1) into the quenching car of the coke blocking car, using water cooling to quench the coke, and sending the cooled lignite coke to a coal mill to grind the particle size to 0.9 to 5.0 mm;

[0040] (3) The ground lignite coke is transported to a fixed-bed gasifier, and a mixture of water vapor and oxygen is introduced into the gasifier from the bottom as a gasifying agent, wherein the mass ratio of lignite coke to water vapor is 1:0.3, and the air-fuel ratio of oxygen to lignite coke is 0.4:1. The gasification temperature of the fixed-bed gasifier is 1000°C. After the reaction is complete and the slag is discharged, 16.92% ash is obtained. The furnace gas is collected through a gas collecting pipe, and the gasifier gas is purified by dry dust removal. The gasifier gas is detected and analyzed by a gas analyzer. The hydrogen content in the gasifier gas is 36.13 vol.%, the carbon monoxide content is 48.11 vol.%, and the carbon dioxide content is 15.76 vol.%. No methane and tar are detected.

[0041] Example 5

[0042] A method for preparing synthesis gas by a two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification comprises the following steps:

[0043] (1) Taking lignite containing 9.56wt% of moisture, 10.40wt% of ash, 29.20wt% of volatile matter and 50.84wt% of fixed carbon as an example, the lignite is ground to 3-10mm, transported to the site by a lignite loading truck to replace coking coal, and added to the carbonization chamber of the coking furnace. After tamping, it is subjected to dry distillation and pyrolysis at 1100°C. After 4 hours, lignite coke is obtained by coking, with a yield of 54.5%. The coke oven gas generated during the dry distillation and pyrolysis process is sent to the bridge pipe through a riser, and then the coke oven gas is collected in the gas collecting pipe. A part of the gas is purified by dry dust removal, and the gas is detected and analyzed by a gas analyzer. The hydrogen content in the coke oven gas is 55.56vol.%, the carbon monoxide content is 34.1vol.%, the carbon dioxide content is 1.83vol.%, and the methane content is 8.51vol.%. The other part of the gas is returned to the return gas main pipe and enters the combustion chamber for combustion;

[0044] (2) using a coke pusher to guide the lignite coke from step (1) into the quenching car of the coke blocking car, using water cooling to quench the coke, and sending the cooled lignite coke to a coal mill to grind the particle size to 0.9 to 5.0 mm;

[0045] (3) The ground lignite coke is transported to a fixed-bed gasifier, and a mixture of water vapor and oxygen is introduced into the gasifier from the bottom as a gasifying agent, wherein the mass ratio of lignite coke to water vapor is 1:0.5, and the air-fuel ratio of oxygen to lignite coke is 0.35:1. The gasification temperature of the fixed-bed gasifier is 1300°C. After the reaction is complete and the slag is discharged, ash of 18.45% is obtained. The furnace gas is collected through a gas collecting pipe, and the gasifier gas is purified by dry dust removal. The gasifier gas is detected and analyzed by a gas analyzer. The hydrogen content in the gasifier gas is 33.77 vol.%, the carbon monoxide content is 49.5 vol.%, and the carbon dioxide content is 16.73 vol.%. No methane and tar are detected.

[0046] The above descriptions are only some embodiments of the present invention, not all embodiments. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification, characterized in that: The specific steps are as follows: (1) grind lignite into fine powder and add it into the carbonization chamber of the coking furnace, tamp it and then perform dry distillation and pyrolysis to obtain lignite coke; (2) The lignite coke is cooled and ground and then transported to a fixed bed gasifier, where water vapor and oxygen are introduced from the bottom as gasifying agents into the fixed bed gasifier. After gasification in the fixed bed gasifier, ash and synthesis gas are obtained.

2. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: Step (1) The lignite particle size is ground to 3-10 mm.

3. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: The temperature of the dry distillation and pyrolysis in step (1) is 600° C. to 1100° C., and the time is 4 to 10 hours.

4. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: Step (2) The lignite coke is ground to a particle size of 0.9 to 5.0 mm.

5. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: The gasification temperature of the fixed bed gasifier in step (2) is 700°C to 1300°C.

6. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: In step (2), the mass ratio of lignite coke to water vapor during the gasification process in the fixed bed gasifier is 1:0.3 to 1:1.

3.

7. The method for preparing synthesis gas by two-step process of coking furnace lignite dry distillation pyrolysis-coke fixed bed gasification according to claim 1, characterized in that: In step (2), the air-fuel ratio of oxygen to lignite coke in the fixed bed gasifier gasification process is 0.1:1 to 0.4:1.