Method for preparing bio-oil by utilizing microwave pyrolysis of waste grease

Copper/biomass porous carbon composite materials were prepared by hydrothermal reaction, and waste oil was pyrolyzed by microwave. This solved the problems of limited deoxygenation capacity and poor stability of catalysts in existing technologies, and achieved the effect of efficient preparation of high-quality bio-oil.

CN118931575AInactive Publication Date: 2024-11-12SHENZHEN GREEN KITCHEN ENVIRONMENTAL PROTECTION PROJECT MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129023.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing technologies, metal oxide catalysts have limited deoxygenation capabilities during the pyrolysis of waste oils, while the small pore size of zeolite molecular sieve catalysts restricts the diffusion of macromolecular compounds, leading to catalyst deactivation. Furthermore, they suffer from poor stability, low yield of organic products, and high yield of polyaromatic hydrocarbons.

Method used

A copper/biomass porous carbon composite material was prepared by forming copper species on the surface of biomass through hydrothermal reaction and combining it with sodium metaphosphate. The copper/biomass porous carbon composite material was then used as a catalyst to promote the pyrolysis of waste oil by microwave pyrolysis.

Benefits of technology

It improved the yield and quality of bio-oil, reduced the reaction temperature, achieved efficient reuse of waste resources, and enhanced the stability and active sites of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931575A_ABST
    Figure CN118931575A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing bio-oil through microwave pyrolysis of waste grease. The method comprises the steps that the waste grease, a microwave absorbent and a copper / biomass porous carbon composite material are mixed and then subjected to pyrolysis under microwaves; collecting liquid oil and gas formed by pyrolysis, and extracting the liquid oil to obtain the bio-oil. Wherein biomass, water-soluble copper salt, a nitrogen source and water are mixed according to the mass ratio of (5-10): (1-2): (0.5-1): (30-80) and then subjected to a hydrothermal reaction, and after the hydrothermal reaction is finished, filtering and drying are conducted to obtain a solid; and calcining the solid to obtain the copper / biomass porous carbon composite material. According to the method, the copper / biomass porous carbon composite material is used as a catalyst, the high-quality bio-oil can be obtained by effectively pyrolyzing the waste grease under the microwave condition, meanwhile, the bio-oil yield is high, the reaction temperature is low, waste resource reutilization can be achieved, and the method is also very suitable for application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste oil recycling, and in particular to a method for preparing bio-oil by utilizing microwave pyrolysis of waste oil. Background Art

[0002] Gasoline, which is mainly composed of hydrocarbon compounds in fossil energy, provides more than 95% of the energy demand of the transportation industry. However, it is a non-renewable resource and will also bring about the problem of greenhouse effect. Exploring green and renewable energy is very important for the energy industry. Waste oil is mostly extracted from food waste generated by the catering industry. It has a wide source and low price. Converting waste oil into biomass fuel can not only alleviate the energy shortage, but also greatly reduce the cost of biomass fuel.

[0003] Some methods have been successfully used to prepare bio-oil using waste oil. CN110102279A discloses a metal-free biochar deoxygenation catalyst and a method for preparing liquid fuel by catalyzing oil compounds using biochar deoxygenation catalyst as a catalyst, and oil compounds are catalytically upgraded in an inert gas atmosphere at a temperature of 300-750°C, and the collected liquid product is liquid fuel. This method realizes the resource utilization of organic materials such as agricultural or urban solid waste and carbohydrates, and also has good catalytic performance for oil compounds. However, this method has a bio-oil yield of more than 60% at temperatures above 550°C. CN116651476A discloses a transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst, which uses zirconium phosphate and transition metal salts as raw materials, adopts the incipient wetness impregnation method to prepare a transition metal-loaded zirconium phosphate oil hydrodeoxygenation catalyst, and the catalyst is mixed with 1-10% of the weight of the biomass oil to be treated in an amount and then subjected to a hydrodeoxygenation reaction at 280-400°C. The catalyst obtained by this method has a bio-oil conversion rate of over 95% under hydrodeoxygenation conditions. However, the hydrogenation reaction has very high requirements for equipment and safety, and is not suitable for popularization and application.

[0004] Microwave-assisted pyrolysis is one of the most eye-catching thermochemical methods developed in recent years. Microwave pyrolysis mainly relies on the interaction between charged particles and electromagnetic radiation, causing violent collisions and friction between molecules to generate heat and thus heat the object. It can greatly reduce the emission of pollutants while providing uniform and rapid heating. There are few reports on the preparation of bio-oil using microwave pyrolysis of waste oils, so it is necessary to construct an effective method. Summary of the invention

[0005] In order to overcome the problems existing in the prior art, the present invention provides a method for preparing bio-oil by microwave pyrolysis of waste oil, comprising: The waste oil, microwave absorbent and copper / biomass porous carbon composite material are mixed and then pyrolyzed under microwave; Liquid oil and gas generated by pyrolysis are collected, and the liquid oil is extracted to obtain bio-oil.

[0006] Currently, metal oxide and zeolite molecular sieve catalysts are more widely used in waste oils and fats. Studies have shown that most transition metal oxide catalysts are beneficial to the formation of alcohols, furans, ketones, acids and phenols in bio-oils, and have a certain catalytic effect on the pyrolysis of waste oils and fats, but their deoxygenation capacity is still limited, making it difficult to prepare high-performance bio-oils. The small pore size of zeolite molecular sieve catalysts limits the diffusion of macromolecular compounds such as polyphenols and long-chain aliphatic hydrocarbons. These compounds will deposit on the surface of the molecular sieve to form coke, leading to catalyst deactivation; at the same time, there are also problems such as poor stability, low yield of organic products, and high yield of polyaromatic hydrocarbons.

[0007] Biomass porous carbon is a porous carbon-rich material, belongs to renewable resources, is environmentally friendly, low-cost, and is a very promising product to replace traditional carbon-based catalysts. The present invention first forms copper species on the surface of biomass by hydrothermal reaction, and biomass will also be initially cracked under the high temperature and high pressure provided by hydrothermal, which is conducive to forming a richer aperture structure in subsequent calcination, and hydrothermal ends to form copper species on the surface of the initially cracked biomass. Subsequently, the copper species are reduced by the formed carbon under a protective gas atmosphere, not only pores are formed on the formed carbon, but also the low-priced copper substances formed are in situ generated on the surface of the carbon matrix to form a composite material with stable structure. However, the pore-forming performance of biomass is poor when only copper ions are introduced, and the low-priced copper species formed may also block the pore structure and reduce the stability of the catalyst. For this reason, sodium metaphosphate is also added during the hydrothermal reaction, which can evenly disperse the copper species, and sodium metaphosphate can also promote the cracking of biomass, which makes it possible to prepare the pore size of the catalyst in the subsequent calcination process and better disperse the low-priced copper formed, thereby improving the reaction active sites of the catalyst. In addition, the introduction of phosphorus doping of sodium metaphosphate and the presence of carbon-phosphorus bonds in the catalyst further improved the catalytic pyrolysis performance.

[0008] Furthermore, the method for preparing the copper / biomass porous carbon composite material comprises: The biomass, water-soluble copper salt, nitrogen source and water are mixed in a mass ratio of 5-10:1-2:0.5-1:30-80 and subjected to hydrothermal reaction, and after the reaction is completed, filtered and dried to obtain a solid; The solid is calcined to obtain a copper / biomass porous carbon composite material.

[0009] Furthermore, after the biomass, water-soluble copper salt, nitrogen source and water are mixed, sodium metaphosphate in an amount of 1 to 3 times the mass of the water-soluble copper salt is added.

[0010] Furthermore, the hydrothermal reaction is continued at 150-180° C. for 2-6 hours.

[0011] Furthermore, the calcination is continued for 1 to 5 hours under a protective gas atmosphere at 500 to 700°C.

[0012] Furthermore, the nitrogen source includes at least one of urea, dicyandiamide and amino acid.

[0013] Preferably, the nitrogen source is selected from amino acids, and the type of amino acids does not need to be strictly limited. For example, it can be at least one of glycine, alanine, valine, leucine, proline, tryptophan, serine, histidine, L-cysteine ​​or their derivatives. As natural biomass, amino acids are one of the most cost-effective and abundant renewable resources, and compared with other nitrogen-containing resources, amino acids have the characteristics of natural degradation and harmless degradation. In addition, even if the amino acid is carbonized at a higher temperature, its product can still maintain a higher nitrogen content, and the nitrogen element can be doped into the product very evenly. The joint introduction of amino acids and sodium metaphosphate is conducive to obtaining nitrogen-containing copper / biomass porous carbon composite materials with larger specific surface area.

[0014] Furthermore, the mass ratio of the waste grease, microwave absorber, and copper / biomass porous carbon composite material is 1-3:20-30:0.2-0.5; The microwave absorber is silicon carbide.

[0015] Furthermore, the pyrolysis under microwave is carried out at a power of 1000-2000 W and a temperature of 300-500° C. for 10-30 min.

[0016] Furthermore, the waste oil includes at least one of expired cooking oil and kitchen waste oil.

[0017] It should be noted that the type of biomass in the present invention does not need to be strictly limited. For example, it can be at least one of rice straw, wheat straw, cotton stalks, corn straw, sugarcane bagasse, and bamboo stalks with a particle size of 200-500 meshes.

[0018] The present invention also provides a bio-oil prepared by the above method.

[0019] Compared with the prior art, the present invention has the following beneficial effects: The present invention prepares preliminary cracked biomass with copper species by hydrothermal reaction, and calcines the preliminary cracked biomass with copper species to prepare a copper / biomass porous carbon composite material with high specific surface area and high active sites. The copper / biomass porous carbon composite material is used as a catalyst to effectively pyrolyze waste oil under microwave conditions to obtain high-quality bio-oil. At the same time, the bio-oil yield is high and the reaction temperature is low, which can realize the recycling of waste resources and is also very suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The XRD patterns of the carbon materials prepared in Examples 1 to 3 and Comparative Example 2 are shown; Figure 2 The scanning electron microscope image of the copper / biomass porous carbon composite material prepared in Example 1 is shown; Figure 3 The scanning electron microscope image of the copper / biomass porous carbon composite material prepared in Example 2 is shown; Figure 4 A scanning electron microscope image of the copper / biomass porous carbon composite material prepared in Example 3 is shown. DETAILED DESCRIPTION

[0021] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0022] Introduction of some raw materials used in the examples and comparative examples of the present invention: Waste oil, collected from a grain and oil company in Hubei, is expired rapeseed oil; Sugarcane bagasse was collected from a sugar factory in Hubei, washed and air-dried, crushed with a grinder and sieved to obtain 300-mesh sugarcane bagasse powder; Silicon carbide, product number A-301, mesh size 100, was purchased from Shijiazhuang Chen Gaoxin Material Technology Co., Ltd.

[0023] The above raw materials and other raw materials not mentioned are all common raw materials. These contents are only to help illustrate the present invention and shall not be construed as strict limitations of the present invention. Those skilled in the art can directly purchase or prepare the same / similar raw materials from the market. These contents will not be repeated in the examples.

[0024] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1 A method for preparing bio-oil by microwave pyrolysis of waste oil, comprising the following steps: S1, 100g of expired rapeseed oil, 2000g of silicon carbide, and 30g of copper / biomass porous carbon composite material were stirred at a speed of 500rpm for 30min to mix evenly, and then transferred to a microwave reactor; S2, start the microwave reactor at a power of 1200 W and a temperature of 350° C. for pyrolysis for 25 min, and use a condenser and an air bag to collect the liquid oil and gas formed during the pyrolysis process; S3. Use 250 mL of carbon dichloride to flush the liquid oil in the condenser, collect it in a conical flask, transfer it to a rotary evaporator at 60° C. to remove carbon dichloride to obtain bio-oil.

[0026] Wherein, the preparation method of the copper / biomass porous carbon composite material is: 10 g of bagasse, 2 g of copper sulfate pentahydrate, 0.8 g of urea, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180° C. for 5 h, filtered after the reaction, and dried in a constant temperature oven at 100° C. for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a copper / biomass porous carbon composite material.

[0027] Example 2 The method is basically the same as Example 1, except that: the preparation method of the copper / biomass porous carbon composite material is: 10 g of bagasse, 2 g of copper sulfate pentahydrate, 0.8 g of urea, 5 g of sodium metaphosphate, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180 °C for 5 h, filtered after the reaction, and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a copper / biomass porous carbon composite material.

[0028] Example 3 The method is basically the same as Example 1, except that: the preparation method of the copper / biomass porous carbon composite material is: 10 g of bagasse, 2 g of copper sulfate pentahydrate, 0.8 g of L-cysteine, 5 g of sodium metaphosphate, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180 °C for 5 h, filtered after the reaction, and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a copper / biomass porous carbon composite material.

[0029] Comparative Example 1 The method is basically the same as Example 1, except that: the preparation method of the copper / biomass porous carbon composite material is: 10 g of bagasse, 2 g of copper sulfate pentahydrate, 5 g of sodium metaphosphate, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180° C. for 5 h, filtered after the reaction, and dried in a constant temperature oven at 100° C. for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a copper / biomass porous carbon composite material.

[0030] Comparative Example 2 A method for preparing bio-oil by microwave pyrolysis of waste oil, comprising the following steps: S1, 100g of expired rapeseed oil, 2000g of silicon carbide, and 30g of biomass porous carbon material were stirred at a speed of 500rpm for 30min to mix evenly, and then transferred to a microwave reactor; S2, start the microwave reactor at a power of 1200 W and a temperature of 350° C. for pyrolysis for 25 min, and use a condenser and an air bag to collect the liquid oil and gas formed during the pyrolysis process; S3. Use 250 mL of carbon dichloride to flush the liquid oil in the condenser, collect it in a conical flask, transfer it to a rotary evaporator at 60° C. to remove carbon dichloride to obtain bio-oil.

[0031] Wherein, the preparation method of biomass porous carbon material is: 10 g of bagasse, 0.8 g of L-cysteine, 5 g of sodium metaphosphate, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180 °C for 5 h, filtered after completion, and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a biomass porous carbon material.

[0032] Comparative Example 3 It is basically the same as Comparative Example 2, except that: the preparation method of the biomass porous carbon material is: 10 g of bagasse and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180 °C for 5 h, filtered and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a biomass porous carbon material.

[0033] Comparative Example 4 It is basically the same as Comparative Example 2, except that: the preparation method of the biomass porous carbon material is: 10 g of bagasse, 0.8 g of L-cysteine, and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor for hydrothermal reaction at 180 °C for 5 h, filtered after completion, and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid; The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a biomass porous carbon material.

[0034] Comparative Example 5 It is basically the same as Comparative Example 2, except that: the preparation method of the biomass porous carbon material is: 10 g of bagasse, 5 g of sodium metaphosphate and 60 g of water were mixed at 300 rpm for 15 min, then transferred to a reactor and hydrothermally reacted at 180 °C for 5 h. After the reaction, the mixture was filtered and dried in a constant temperature oven at 100 °C for 16 h to obtain a solid. The solid was calcined in a nitrogen atmosphere tube furnace at 650°C for 2 h, then naturally cooled to room temperature, and the black powder was washed three times with ethanol and water respectively, and dried in a constant temperature oven at 120°C for 12 h to obtain a biomass porous carbon material.

[0035] Test Case The nitrogen isothermal adsorption-desorption curves of the carbon materials in the embodiments and comparative examples were tested to obtain the specific surface areas. The results are shown in Table 1.

[0036] Table 1 Specific surface area of ​​carbon materials

[0037] From the test results of Table 1, it can be seen that among the biomass porous carbon materials of Comparative Examples 2 to 5, Comparative Example 3, which did not add nitrogen source and sodium metaphosphate in the early hydrothermal treatment, has the smallest specific surface area; Comparative Example 4, which introduced L-cysteine ​​alone, and Comparative Example 5, which introduced sodium metaphosphate, have significantly increased specific surface areas, and Comparative Example 2, which introduced L-cysteine ​​and sodium metaphosphate together, has the largest specific surface area. This rule is also consistent with the copper / biomass porous carbon composite material prepared in Examples 1 to 3 and Comparative Example 1. This is because the introduction of a nitrogen source can promote the decomposition of biomass that is initially cracked by hydrothermal treatment under high-temperature calcination, producing more aperture structures, and the groups in sodium metaphosphate can promote the cracking of biomass, and can also introduce phosphorus doping during calcination to further promote the decomposition of generated carbon and introduce more aperture structures. It also illustrates that the joint introduction of L-cysteine ​​and sodium metaphosphate has a good synergistic effect and improves the specific surface area of ​​the carbon material. In the copper / biomass porous carbon composite materials prepared in Examples 1 to 3 and Comparative Example 1, the hydrothermal reaction forms copper species on the surface of the cracked biomass. At high temperatures, the copper species are not very etching for the formed carbon and may even block the pores. Among them, Example 3 has a larger specific surface area because the presence of L-cysteine ​​and sodium metaphosphate can better disperse the copper species generated by the hydrothermal reaction.

[0038] The carbon materials prepared in the examples and comparative examples were observed by XRD. Figure 1 As shown. It can be seen that comparative example 2 shows broad diffraction peaks at 23° and 43°, corresponding to the (002) and (100) crystal planes of carbon, respectively. Examples 1 to 3 have similar diffraction peaks. In addition to the (002) and (100) crystal planes of carbon, the diffraction peaks at 29.5°, 36.7°, 42.3° and 61.8° correspond to the (110), (111), (200) and (220) crystal planes of Cu2O, respectively. The remaining diffraction peaks at 43.5°, 50.9° and 74.2° are the (111), (200) and (311) crystal planes of Cu, respectively. These results illustrate the successful preparation of low-cost copper / carbon composite materials.

[0039] The microscopic morphology of the copper / biomass porous carbon composite materials prepared in Examples 1 to 3 was observed using a scanning electron microscope. It can be clearly seen that the low-cost copper particles in the material prepared in Example 3 are finer, more evenly dispersed, and less agglomerated.

[0040] The bio-oil produced in the embodiment and the comparative example was injected into the gas-mass spectrometer and the inlet temperature was maintained at 280°C. 99.99% helium was used as the carrier gas at a flow rate of 0.6 mL / min. The NIST database was used for peak identification to determine the type of oil product produced. The gas produced in the embodiment and the comparative example was used in a GC9790Ⅱ gas chromatograph, where H 2 , O2 、N 2 ,CO,CO 2 and CH 4 The analysis was performed using an MS5A column, and other hydrocarbon gases were analyzed using a ProapakQ column. These results are shown in Table 2, where only the fuel-related products are listed for bio-oil, and only the main H 2 , CO 2 and CH 4 volume share.

[0041] Table 2 Composition results

[0042]

[0043] From the test results in Table 2, it can be seen that the copper / biomass porous carbon composite materials prepared in Examples 1 to 3 and Comparative Example 1 have higher conversion rates than the biomass porous carbon prepared in Comparative Examples 2 to 5. 5 ~C 16 Higher aliphatic hydrocarbon yields and lower C 5 ~C 16 The yield of aliphatic hydrocarbons and alcohols; the H 2 and CH 4 The volume proportion is higher, which is derived from the good catalytic effect of low-valent copper and the biomass porous carbon as a good matrix to provide catalytic stability. At the same time, because the introduction of phosphorus doping of sodium metaphosphate and nitrogen doping of L-cysteine, sodium metaphosphate and L-cysteine ​​not only promote the initial cracking of biomass but also enhance the dispersion of copper species formed, so that the low-valent copper formed by calcination is well dispersed, and the presence of carbon-phosphorus bonds in carbon materials further improves the catalytic pyrolysis performance. Therefore, Example 3 has the highest conversion rate, and the bio-oil obtained has higher oil quality and a lower alcohol proportion.

[0044] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing bio-oil by microwave pyrolysis of waste oil, characterized in that: include, The waste oil, microwave absorbent and copper / biomass porous carbon composite material are mixed and then pyrolyzed under microwave; Liquid oil and gas generated by pyrolysis are collected, and the liquid oil is extracted to obtain bio-oil.

2. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 1, characterized in that: The method for preparing the copper / biomass porous carbon composite material comprises: The biomass, water-soluble copper salt, nitrogen source and water are mixed in a mass ratio of 5-10:1-2:0.5-1:30-80 and subjected to hydrothermal reaction, and after the reaction is completed, filtered and dried to obtain a solid; The solid is calcined to obtain a copper / biomass porous carbon composite material.

3. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 2, characterized in that: After mixing biomass, water-soluble copper salt, nitrogen source and water, sodium metaphosphate in an amount of 1 to 3 times the mass of the water-soluble copper salt is added.

4. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 2, characterized in that: The hydrothermal reaction is continued at 150-180° C. for 2-6 hours.

5. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 2, characterized in that: The calcination is continued for 1 to 5 hours under a protective gas atmosphere at 500 to 700°C.

6. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 2, characterized in that: The nitrogen source includes at least one of urea, dicyandiamide and amino acid.

7. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 1, characterized in that: The mass ratio of the waste grease, microwave absorber and copper / biomass porous carbon composite material is 1-3:20-30:0.2-0.5; The microwave absorber is silicon carbide.

8. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 1, characterized in that: The microwave pyrolysis is carried out at a power of 1000-2000 W and a temperature of 300-500° C. for 10-30 min.

9. The method for preparing bio-oil by microwave pyrolysis of waste oil according to claim 1, characterized in that: The waste grease includes at least one of expired edible oil and kitchen waste grease.

10. A bio-oil, characterized in that: The method is prepared by any one of claims 1 to 9.