Pneumatic grading-strong magnetic tailing discarding-suspension roasting system for iron ore and use method of pneumatic grading-strong magnetic tailing discarding-suspension roasting system
Through pneumatic grading and strong magnetic tailing throwing technology, the coarse and fine ore of iron ore are graded and processed. Combined with suspended roasting technology, the problem of low-grade iron ore resource treatment efficiency is solved, and efficient iron ore resource utilization and high quality are achieved Recycling of grade iron concentrate.
Patent Information
- Application Number
- CN202410980218.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
my country's iron ore resources are mainly low-grade weak magnetic ore, which leads to long process during the treatment process, high grinding unit consumption, high selection cost and poor product indicators, which cannot meet the domestic demand for iron ore and must rely on foreign countries. import.
Using pneumatic grading-strong magnetic tail-suspended and suspended roasting system, coarse ore materials are separated by pneumatic grading. Coarse ore materials are mixed with fine ore materials after grinding and weak magnetic separation. Combined with suspension roasting technology, iron ore is calcined. Stone is converted into high-grade harsh magnetic iron ore, reducing the amount of roasted ore feeding, and improving system energy efficiency and ore quality.
The recycling of high-quality iron concentrate products with iron grades greater than 65% has been achieved, and the total iron recovery rate has reached more than 90%, reducing system energy consumption and grinding costs, and improving the utilization efficiency of iron ore resources.
Smart Images

Figure CN118932170A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mineral processing, and in particular to an iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system and a use method thereof. Background Art
[0002] Since 2005, with the continuous development of my country's economy, the demand for steel in various industries has increased, and therefore the demand for iron ore has increased year by year. my country's overall iron ore reserves are rich, but they cannot meet my country's demand for iron ore. It can only rely on foreign imports. my country's annual imports of iron ore have remained high all year round, once exceeding 1 billion tons. The high dependence on imports of iron ore has had a serious impact on the healthy development of my country's steel industry and the national economy.
[0003] my country's iron ore resources are mainly low-grade hematite, limonite, siderite, specularite and other weakly magnetic ores. Domestic processing of weakly magnetic iron ore has problems such as long process, high grinding unit consumption, high separation cost and poor product indicators, which makes the cost of domestic iron ore high and the market competitiveness insufficient, so it has to rely on imports all year round.
[0004] Traditional iron ore separation processes include grinding, magnetic separation, gravity separation, flotation, etc. Suspended magnetization roasting technology, as an emerging technology, can transform weakly magnetic iron minerals into strong magnetic iron minerals under certain temperature and atmosphere conditions, so that iron ore can be efficiently recovered using weak magnetism. Since roasting technology consumes heat energy, the grade of domestic iron ore is generally low, so there is a large heat consumption, which has a certain impact on the efficient utilization of iron ore. Summary of the invention
[0005] In view of the above problems, the present invention provides an iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system and a use method. The iron ore can be classified into coarse and fine ore materials by pneumatic classification. The coarse ore materials are mixed with fine ore materials after grinding, weak magnetic separation and strong magnetic tailings discarding as roasting feed ore, which reduces the roasting feed amount, improves the roasting feed grade, reduces system energy consumption, and improves the quality of the roasted ore. The roasted ore is subjected to grinding-magnetic separation to finally obtain a high-quality iron concentrate product with an iron grade greater than 65%, and the total iron recovery rate reaches more than 90%.
[0006] The iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system of the present invention comprises the following subsystems: a pneumatic classification subsystem, a first magnetic separation subsystem, a suspension roasting subsystem, and a second magnetic separation subsystem;
[0007] The pneumatic classification subsystem includes a pneumatic classification device, a fourth gas-solid separator, and a first dust removal device; the first magnetic separation subsystem includes a first weak magnetic separator and a strong magnetic separator; the suspension roasting subsystem includes a suspension roasting device and a first gas-solid separator;
[0008] The top air outlet of the pneumatic classification device is connected to the feed port of the fourth gas-solid separator, the air outlet of the fourth gas-solid separator is connected to the air inlet of the first dust removal device, the discharge port of the fourth gas-solid separator and the discharge port of the first dust removal device are both connected to the feed port of the first gas-solid separator; the bottom discharge port of the pneumatic classification device is connected to the feed port of the first weak magnetic separator; the concentrate discharge port of the first weak magnetic separator and the concentrate discharge port of the high-intensity magnetic separator are both connected to the feed port of the first gas-solid separator, and the tailings discharge port of the first weak magnetic separator is connected to the feed port of the high-intensity magnetic separator; the discharge port of the first gas-solid separator is connected to the feed port of the suspension roasting device; the suspension roasting subsystem is connected to the second magnetic separation subsystem.
[0009] The suspension roasting subsystem includes a suspension roasting device, a first gas-solid separator, a second dust removal device, a second gas-solid separator, a reduction reactor, a third gas-solid separator, and a third material storage device;
[0010] The discharge port of the first gas-solid separator is connected to the feed port of the suspension roasting device, the discharge port of the suspension roasting device is connected to the feed port of the second gas-solid separator, the gas outlet of the second gas-solid separator is connected to the gas inlet of the first gas-solid separator, the discharge ports of the second gas-solid separator, the reduction reactor, and the third gas-solid separator are connected to the feed port in sequence; the gas outlet of the third gas-solid separator is connected to the gas inlet of the suspension roasting device;
[0011] The discharge port of the fourth gas-solid separator, the discharge port of the first dust removal device, the concentrate discharge port of the first weak magnetic separator, and the concentrate discharge port of the high-intensity magnetic separator are all connected to the feed port of the third material storage device; the discharge port of the third material storage device is connected to the feed port of the first gas-solid separator; the air outlet of the third material storage device is connected to the air inlet of the second dust removal device; the discharge port of the second dust removal device is connected to the feed port of the first gas-solid separator; the discharge port of the third gas-solid separator is connected to the second magnetic separation subsystem.
[0012] The second magnetic separation subsystem includes a slurry pool, a second grinding equipment, and a second weak magnetic separator;
[0013] The discharge port of the third gas-solid separator is connected to the feed port of the slurry pool, and the discharge ports of the slurry pool, the second grinding equipment, and the second weak magnetic separator are connected to the feed port in sequence.
[0014] The iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system of the present invention includes the following specific equipment and connection methods:
[0015] Air force classification subsystem:
[0016] The discharge port of the raw material silo, the jaw crusher, the first high-pressure roller mill, the first screw feeder, and the feed port of the pneumatic classifier are connected in sequence; the air inlet of the pneumatic classifier is connected with the air outlet of the high-pressure air supply device through a pipeline, the bottom discharge port of the pneumatic classifier is connected with the feed port of the first material storage device through a pipeline, the top discharge port of the pneumatic classifier is connected with the feed port of the fourth gas-solid separator through a pipeline, the bottom discharge port of the fourth gas-solid separator is connected with the feed port of the third material storage device through a belt, the air outlet of the fourth gas-solid separator is connected with the air inlet of the first dust removal device through a pipeline, the discharge port of the first dust removal device is connected with the feed port of the third material storage device through a belt, and the air outlet of the first dust removal device is connected with the chimney through a pipeline.
[0017] The first magnetic separation system:
[0018] The discharge ports and feed ports of the first material storage device, the second high-pressure roller mill, the first grinding equipment, and the first weak magnetic separator are connected in sequence; the concentrate discharge port of the first weak magnetic separator is connected to the feed port of the first filter press through a pipeline, the tailings discharge port of the first weak magnetic separator is connected to the feed port of the first concentrator through a pipeline, the discharge port of the first concentrator is connected to the feed port of the high-intensity magnetic separator through a pipeline, the concentrate discharge port of the high-intensity magnetic separator is connected to another feed port of the first filter press through a pipeline, the discharge port of the first filter press is connected to the feed port of the second material storage device through a belt, and the discharge port of the second material storage device is connected to the feed port of the third material storage device through a belt.
[0019] Suspension roasting subsystem:
[0020] The discharge port of the third material storage device is connected with the feed port of the second screw feeder through a pipeline, the air inlet of the third material storage device is connected with the air outlet of the first gas-solid separator through a pipeline, the air outlet of the third material storage device is connected with the air inlet of the second dust removal device through a pipeline, the air outlet of the second dust removal device is connected with the chimney through a negative pressure fan, and the discharge port of the second dust removal device is connected with the feed port of the second screw feeder through a pipeline; the discharge port of the second screw feeder is connected with the feed port of the first gas-solid separator through a pipeline, the discharge port of the first gas-solid separator is connected with the feed port of the suspension roasting device through a pipeline, the discharge port of the suspension roasting device is connected with the feed port of the second gas-solid separator through a pipeline, and the air outlet of the second gas-solid separator is connected with the air inlet of the first gas-solid separator through a pipeline; the discharge ports and feed ports of the second gas-solid separator, the reduction reactor, and the third gas-solid separator are connected in sequence; the air outlet of the third gas-solid separator is connected with the air inlet of the suspension roasting device through a pipeline.
[0021] The second magnetic separation system:
[0022] The discharge port and feed port of the third gas-solid separator, the slurry pool, the second grinding equipment and the second weak magnetic separator are connected in sequence; the concentrate discharge port of the second weak magnetic separator is connected with the feed port of the second filter press through a pipeline, and the discharge port of the second filter press is connected with the feed port of the fourth material storage device through a belt; the tailings discharge port of the second weak magnetic separator is connected with another feed port of the second concentrator through a pipeline, and the discharge port of the second concentrator is connected with the feed port of the fifth material storage device through a pipeline.
[0023] The suspension roasting device, gas-solid separator, reduction reactor and dust removal device in the system are all equipped with thermocouple temperature measuring devices and pressure sensor devices, which can monitor and record the temperature of each temperature measuring point and the pressure of each pressure measuring point in real time through a computer.
[0024] The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system of the present invention comprises the following steps:
[0025] S1 Pneumatic classification: The ore after iron ore crushing is fed into the pneumatic classification device. After the ore is processed by the pneumatic classification device, a gas phase containing fine-grained ore and a solid phase containing coarse-grained ore are obtained; the gas phase enters the fourth gas-solid separator to separate fine-grained ore and fine ore gas, the fine-grained ore is fed into the first gas-solid separator, the fine ore gas is processed by the first dust removal device, and the collected ore is fed into the first gas-solid separator, and the solid phase containing coarse-grained ore is crushed and fed into the first weak magnetic separator;
[0026] S2 strong magnetic tailings discarding: the first weak magnetic separator separates the first weak magnetic concentrate and the first weak magnetic tailings; the first weak magnetic tailings are fed into the strong magnetic separator, and the strong magnetic separator separates the strong magnetic concentrate and the strong magnetic tailings; the first weak magnetic concentrate and the strong magnetic concentrate are fed into the first gas-solid separator;
[0027] S3 Suspension roasting: the ore separated by the first gas-solid separator is fed into the suspension roasting device for suspension roasting, and the roasted ore is fed into the second magnetic separation subsystem;
[0028] S4 Magnetic Separation after Roasting: The ore after roasting is separated into iron concentrate products and tailings by the second magnetic separation subsystem;
[0029] The classification particle size of the pneumatic classifier is 3mm; the iron grade of the iron ore is 20%-35%, the particle size is 10-20mm; the crushing particle size is 5-8mm; the crushing particle size of the coarse-grained ore is 3mm, and the content of the -200 mesh after crushing is 40%-60%; the magnetic field strength of the first weak magnetic separator is 0.1-0.3T; the magnetic field strength of the strong magnetic separator is 0.4-0.6T;
[0030] The suspension roasting includes igniting natural gas and air and then passing them into a suspension roasting device, so that the temperature of the device is 600-700°C, and the ore is heated to 500-540°C during roasting.
[0031] The S3 suspension roasting includes the following specific steps: after the ore is roasted in the suspension roasting device, it is fed into the second gas-solid separator to separate the roasted ore and the roasting gas, the roasting gas is fed into the first gas-solid separator, the roasted ore is reduced in the reduction reactor and then fed into the third gas-solid separator to separate the reduced ore and the reducing gas, the reduced ore is fed into the second magnetic separator system, and the reducing gas is fed into the suspension roasting device;
[0032] The gas separated by the first gas-solid separator is fed into the third material storage device to preheat the ore once, the preheated ore and the ore collected by the second dust removal device are both fed into the first gas-solid separator, and exchange heat with the roasting gas fed into the first gas-solid separator for secondary preheating and gas-solid separation, the separated ore is fed into the suspension roasting device for roasting, and the separated gas is fed into the third material storage device to preheat the ore once;
[0033] After the primary preheating, the temperature of the ore is 100-200°C, and the gas is cooled to 150-300°C; after the secondary preheating, the temperature of the ore is 200-300°C, and the gas is cooled to 300-400°C; the reducing gas for the reduction reaction is hydrogen or carbon monoxide, the reducing gas concentration is 20%-40%, and the reaction time is 10-30 minutes;
[0034] The S4 post-roasting magnetic separation includes the following specific steps: grinding the roasted ore and feeding it into a second weak magnetic separator for magnetic separation to obtain a second weak magnetic concentrate and a second weak magnetic tailings; the ore particle size after grinding is -200 mesh and the content is 50%-80%.
[0035] The application of the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system of the present invention comprises the following specific steps:
[0036] S1 Pneumatic classification: Iron ore of a certain particle size enters the raw material silo, the iron grade of the ore is 20%-35%, and the particle size is 10-20mm. The ore in the raw material silo enters the jaw crusher and the first high-pressure roller mill in turn through the belt through the discharge port for crushing, and the crushing particle size is 5-8mm. The crushed ore enters the pneumatic classification device through the first screw feeder. The gas flow rate at the outlet of the high-pressure air supply device is adjusted according to the classification particle size set by the system, and the classification particle size is 3mm; the ore is classified by the pneumatic classification device to obtain coarse-grained ore and fine-grained ore. The fine-grained ore enters the fourth gas-solid separator with the gas through the top discharge port of the pneumatic classification device for gas-solid separation. The gas in the fourth gas-solid separator is purified by the first dust removal device and discharged into the atmosphere through the chimney.
[0037] S2 Strong Magnetic Tailings: The coarse-grained ore treated by the pneumatic classifier enters the first material storage device, the second high-pressure roller mill, the first grinding equipment and the first weak magnetic separator in sequence. The crushing particle size range of the second high-pressure roller mill is controlled to be 3mm, the particle size range of the first grinding equipment is -200 mesh with a content of 40% to 60%, and the magnetic field strength range of the first weak magnetic separator is 0.1 to 0.3T;
[0038] The first weak magnetic tailings produced by the first weak magnetic separator are concentrated by the first concentrator and then enter the strong magnetic separator. The magnetic field strength of the strong magnetic separator is 0.4-0.6T. The first weak magnetic concentrate produced by the first weak magnetic separator and the strong magnetic concentrate produced by the strong magnetic separator are mixed and processed by the first filter press device and then enter the second material storage device, and the strong magnetic tailings are separated at the same time.
[0039] S3 Suspension roasting: the ore in the second material storage device is mixed with the ore in the fourth gas-solid separator and the first dust removal device and then enters the third material storage device; the ore in the third material storage device is preheated and dried by the hot gas of the first gas-solid separator and then enters the second screw feeder, the ore is preheated and dried and heated to 100-200°C, and the gas is cooled to 150-300°C; the gas that has completed the heat exchange is cooled and purified by the second dust removal device and then discharged into the atmosphere through the chimney by the negative pressure fan, and the gas cooling temperature is 30-60°C; the ore produced by the second dust removal device is the same as that after drying The ore is fed into the second screw feeder together with the ore of the second gas-solid separator; the second screw feeder feeds the ore according to the system setting feeding amount together with the hot gas of the second gas-solid separator into the first gas-solid separator to complete the secondary preheating, the ore is preheated to 200-300°C by the hot gas, and the hot gas that completes the heat exchange is cooled to 300-400°C; the preheated ore enters the suspension roasting device through the bottom discharge port of the first gas-solid separator for suspension roasting, natural gas and air are introduced into the suspension roasting device and ignited, the temperature in the stable device is 600-700°C, and the ore is heated to 500-540°C;
[0040] The roasted ore and flue gas enter the second gas-solid separator through the top discharge port of the suspension roasting device to separate the roasted ore and the roasting gas. The roasted ore enters the reduction reactor to complete the reduction reaction, wherein the reducing gas is hydrogen or carbon monoxide, the reducing gas concentration is 20% to 40%, and the reaction time is 10 to 30 minutes; the roasting gas enters the first gas-solid separator through the top discharge port of the second gas-solid separator to preheat the ore, and the roasting gas temperature is 400 to 500°C; the ore reduced in the reduction reactor is cooled and gas-solid separated in the third gas-solid separator to separate the reduced ore and the reducing gas, and the reducing gas enters the suspension roasting device for combustion; the reduced ore enters the slurry pool.
[0041] S4 Magnetic separation after roasting: The reduced ore enters the slurry pool to be prepared into a slurry of a certain concentration and then enters the second grinding equipment for grinding. The mass concentration of the slurry is controlled to be 40% to 70%. The fineness of the ore after grinding in the second grinding equipment is controlled to be 50% to 80% at -200 mesh. The grinding product is processed by the second weak magnetic separator to obtain a second weak magnetic concentrate and a second weak magnetic tailings. The second weak magnetic concentrate is filtered by the second filter press and then enters the fourth material storage device. The second weak magnetic tailings are processed by the second concentrator together with the strong magnetic tailings produced by the strong magnetic separator and then enter the fifth material storage device.
[0042] Compared with the existing magnetic roasting and separation processes, the present invention adopts a combination of pneumatic classification-strong magnetic tailings discarding and suspended magnetic roasting to discard part of the qualified tailings in advance, thereby reducing the roasting processing volume. Without reducing the iron recovery rate, the energy consumption of the system is reduced, the quality of the roasted ore and iron concentrate is improved, and the quality of the ore is optimized. At the same time, the energy consumption of grinding is reduced, and iron concentrate with higher indicators is obtained, which can be used as a high-grade raw material for operations such as sintering pellets, thereby realizing efficient utilization of iron ore resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The present invention is a process flow chart of the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system.
[0044] In the figure: 1-raw material silo, 2-jaw crusher, 3-first high pressure roller mill, 4-first screw feeder, 5-pneumatic classifier, 6-high pressure air supply device, 7-first material storage device, 8-second high pressure roller mill, 9-first grinding equipment, 10-first weak magnetic separator, 11-first concentration device, 12-strong magnetic separator, 13-first filter press, 14-second material storage device, 15-third material storage device, 16-second screw feeder, 17-first a gas-solid separator, 18-suspension roasting device, 19-a second gas-solid separator, 20-a reduction reactor, 21-a third gas-solid separator, 22-a slurry pool, 23-a second grinding equipment, 24-a second weak magnetic separator, 25-a second filter press device, 26-a fourth material storage device, 27-a second concentration device, 28-a fifth material storage device, 29-a fourth gas-solid separator, 30-a first dust removal device, 31-a second dust removal device, 32-a negative pressure fan, 33-a chimney. DETAILED DESCRIPTION
[0045] The process flow of the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system of the present invention is as follows: Figure 1 shown.
[0046] Example 1
[0047] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of siderite, and the raw material iron grade is 34.05%. The method is carried out in the following steps:
[0048] S1 Pneumatic classification: Iron ore with a maximum particle size of 20 mm enters the raw material silo 1, and the ore in the raw material silo 1 enters the jaw crusher 2 and the first high-pressure roller mill 3 in sequence through the discharge port through the belt for crushing, and the crushing particle size is 8 mm. The crushed ore enters the pneumatic classification device 5 through the first screw feeder 4, and the gas flow rate at the outlet of the high-pressure air supply device 6 is adjusted according to the classification particle size set by the system, and the classification particle size is 3 mm; the ore is processed by the pneumatic classification device 5 to obtain coarse-grained ore and fine-grained ore, and the iron grade of the coarse-grained ore is 26.14%, and the iron grade of the fine-grained ore is 44.57%; the fine-grained ore enters the fourth gas-solid separator 29 with the gas through the top discharge port of the pneumatic classification device 5 for gas-solid separation, and the gas in the fourth gas-solid separator 29 is purified by the first dust removal device 30 and discharged into the atmosphere through the chimney 33;
[0049] S2 Strong magnetic tailings: The coarse-grained ore treated by the pneumatic classifier 5 enters the first material storage device 7, the second high-pressure roller mill 8, the first grinding equipment 9 and the first weak magnetic separator 10 in sequence. The crushing particle size range of the second high-pressure roller mill 8 is controlled to be 3mm, the discharge particle size of the first grinding equipment 9 is -200 mesh and the content is 40%, and the magnetic field strength of the first weak magnetic separator 10 is 0.3T;
[0050] The first weak magnetic tailings produced by the first weak magnetic separator 10 are concentrated by the first concentrator 11 and then enter the strong magnetic separator 12. The magnetic field strength of the strong magnetic separator is 0.6T. The first weak magnetic concentrate produced by the first weak magnetic separator 10 and the strong magnetic concentrate produced by the strong magnetic separator 12 are mixed and processed by the first filter press 13 and then enter the second material storage device 14. At the same time, the strong magnetic tailings are separated. The iron grade of the strong magnetic tailings is 6.15%, and the iron recovery rate is 4.91%;
[0051] S3 suspension roasting: the ore in the second material storage device 14 is mixed with the ore in the fourth gas-solid separator 29 and the first dust removal device 30 and then enters the third material storage device 15;
[0052] The ore in the third material storage device 15 is preheated and dried by the hot gas of the first gas-solid separator 17 and then enters the second screw feeder 16. The ore is preheated and dried and heated to 200°C, and the gas is cooled to 300°C. The gas that has completed the heat exchange is cooled and purified by the second dust removal device 31 and then discharged into the atmosphere through the chimney 33 by the negative pressure fan 32. The gas cooling temperature is 60°C. The ore produced by the second dust removal device 31 enters the second screw feeder 16 together with the dried ore. The second screw The feeder 16 feeds the ore material into the first gas-solid separator 17 together with the hot gas from the second gas-solid separator 19 according to the system set feeding amount to complete the secondary preheating. The ore material is preheated to 300°C by the hot gas for the secondary preheating, and the hot gas after the heat exchange is cooled to 400°C. The preheated ore material enters the suspension roasting device 18 through the bottom discharge port of the first gas-solid separator 17 for suspension roasting. Natural gas and air are introduced into the suspension roasting device and ignited to stabilize the temperature in the device at 700°C, and the ore material is heated to 540°C.
[0053] The roasted ore enters the second gas-solid separator 19 through the top discharge port of the suspended roasting device 18, and the roasted ore and the roasting gas are separated by the second gas-solid separator 19. The roasted ore enters the reduction reactor 20 to complete the reduction reaction, wherein the reducing gas is hydrogen, the reducing gas concentration is 40%, and the reaction time is 30 minutes; the roasting gas enters the first gas-solid separator 17 through the top gas outlet of the second gas-solid separator 19 to preheat the ore, and the roasting gas temperature is 500°C; the ore reduced by the reduction reactor 20 is cooled and gas-solid separated by the third gas-solid separator 21, and the reduced ore and the reducing gas are separated, and the reducing gas enters the suspended roasting device 18 for combustion; the reduced ore enters the slurry pool.
[0054] S4 Magnetic separation after roasting: The reduced ore enters the slurry pool 22 and is prepared into a slurry of a certain concentration, and then enters the second grinding equipment 23 for grinding. The mass concentration of the slurry is controlled to be 70%, and the fineness of the ore after grinding by the second grinding equipment is controlled to be -200 mesh and 50%. The grinding product is processed by the second weak magnetic separator 24 to obtain a second weak magnetic concentrate and a second weak magnetic tailings. The iron grade of the second weak magnetic concentrate is 66.42%, the iron recovery rate is 90.37%, and the iron grade of the second weak magnetic tailings is 7.02%; the second weak magnetic concentrate is filtered by the second filter press 25 and then enters the fourth material storage device 26. The second weak magnetic tailings are processed by the second concentrator 27 together with the strong magnetic tailings produced by the strong magnetic separator 12 and then enter the fifth material storage device 28.
[0055] Example 2
[0056] The main iron minerals of the iron ore in this embodiment are hematite and a small amount of limonite, and the raw material iron grade is 28.44%. The method is the same as that of Example 1, except for the following:
[0057] S1 Pneumatic classification: The maximum particle size of the iron ore entering the raw material silo 1 is 15 mm; the crushing particle size of the first high-pressure roller mill 3 is 7 mm; after the ore is processed by the pneumatic classification device 5, the iron grade of the coarse-grained ore is 22.06%, and the iron grade of the fine-grained ore is 36.47%.
[0058] S2 strong magnetic tailings discarding: the discharge particle size of the first grinding equipment 9 is -200 mesh and the content is 50%, the magnetic field strength of the first weak magnetic separator 10 is 0.2T; the magnetic field strength of the strong magnetic separator is 0.5T; the iron grade of the strong magnetic tailings is 4.80%, and the iron recovery rate is 3.87%.
[0059] S3 suspension roasting: after the primary preheating, the ore is heated to 150°C, and the gas is cooled to 250°C; the gas temperature discharged into the atmosphere through the chimney 33 is 50°C; after the secondary preheating, the ore is heated to 250°C, and the gas is cooled to 350°C; the temperature in the suspension roasting device is 650°C, and the ore is heated to 520°C;
[0060] The reducing gas in the reduction reactor 20 is carbon monoxide, the reducing gas concentration is 30%, and the reaction time is 20 minutes; the temperature of the roasting gas discharged from the top outlet of the second gas-solid separator 19 and entering the first gas-solid separator 17 is 450°C.
[0061] S4 Magnetic separation after roasting: The mass concentration of slurry in the slurry pool 22 is 50%, and the fineness of the ore after grinding by the second grinding equipment is -200 mesh and the content is 65%; the iron grade of the weak magnetic concentrate separated by the second weak magnetic separator 24 is 65.45%, the iron recovery rate is 90.08%, and the iron grade of the weak magnetic tailings is 4.72%.
[0062] Example 3
[0063] The main iron minerals of the iron ore in this embodiment are hematite, limonite and a small amount of specularite, and the raw material iron grade is 22.34%. The method is the same as that of Example 1, except for the following:
[0064] S1 Pneumatic classification: The maximum particle size of the iron ore entering the raw material silo 1 is 12 mm; the crushing particle size of the first high-pressure roller mill 3 is 5 mm; after the ore is processed by the pneumatic classification device 5, the iron grade of the coarse-grained ore is 16.78%, and the iron grade of the fine-grained ore is 30.55%.
[0065] S2 strong magnetic tailings discarding: the discharge particle size of the first grinding equipment 9 is -200 mesh and the content is 60%, the magnetic field strength of the first weak magnetic separator 10 is 0.1T; the magnetic field strength of the strong magnetic separator is 0.4T; the iron grade of the strong magnetic tailings is 3.45%, and the iron recovery rate is 4.43%.
[0066] S3 suspension roasting: after the primary preheating, the ore is heated to 100°C, and the gas is cooled to 150°C; the temperature of the gas discharged into the atmosphere through the chimney 33 is 30°C; after the secondary preheating, the ore is heated to 200°C, and the gas is cooled to 300°C; the temperature in the suspension roasting device is 600°C, and the ore is heated to 500°C;
[0067] The reducing gas in the reduction reactor 20 is a mixed gas (hydrogen: carbon monoxide = 3:1), the reducing gas concentration is 20%, and the reaction time is 10 minutes; the roasting gas temperature discharged from the top outlet of the second gas-solid separator 19 and entering the first gas-solid separator 17 is 400°C.
[0068] S4 Magnetic separation after roasting: The mass concentration of slurry in the slurry pool 22 is 40%, and the fineness of the ore after grinding by the second grinding equipment is -200 mesh content 80%; the iron grade of the weak magnetic concentrate separated by the second weak magnetic separator 24 is 65.05%, the iron recovery rate is 90.16%, and the iron grade of the weak magnetic tailings is 3.58%.
Claims
1. An iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system, characterized in that: Includes the following subsystems: Pneumatic classification subsystem, first magnetic separation subsystem, suspension roasting subsystem, second magnetic separation subsystem; The pneumatic classification subsystem includes a pneumatic classification device, a fourth gas-solid separator, and a first dust removal device; the first magnetic separation subsystem includes a first weak magnetic separator and a strong magnetic separator; the suspension roasting subsystem includes a suspension roasting device and a first gas-solid separator; The top air outlet of the pneumatic classification device is connected to the feed port of the fourth gas-solid separator, the air outlet of the fourth gas-solid separator is connected to the air inlet of the first dust removal device, the discharge port of the fourth gas-solid separator and the discharge port of the first dust removal device are both connected to the feed port of the first gas-solid separator; the bottom discharge port of the pneumatic classification device is connected to the feed port of the first weak magnetic separator; the concentrate discharge port of the first weak magnetic separator and the concentrate discharge port of the high-intensity magnetic separator are both connected to the feed port of the first gas-solid separator, and the tailings discharge port of the first weak magnetic separator is connected to the feed port of the high-intensity magnetic separator; the discharge port of the first gas-solid separator is connected to the feed port of the suspension roasting device; the suspension roasting subsystem is connected to the second magnetic separation subsystem.
2. The iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 1 is characterized in that: The suspension roasting subsystem includes a suspension roasting device, a first gas-solid separator, a second dust removal device, a second gas-solid separator, a reduction reactor, a third gas-solid separator, and a third material storage device; The discharge port of the first gas-solid separator is connected to the feed port of the suspension roasting device, the discharge port of the suspension roasting device is connected to the feed port of the second gas-solid separator, the gas outlet of the second gas-solid separator is connected to the gas inlet of the first gas-solid separator, the discharge ports of the second gas-solid separator, the reduction reactor, and the third gas-solid separator are connected to the feed port in sequence; the gas outlet of the third gas-solid separator is connected to the gas inlet of the suspension roasting device; The discharge port of the fourth gas-solid separator, the discharge port of the first dust removal device, the concentrate discharge port of the first weak magnetic separator, and the concentrate discharge port of the high-intensity magnetic separator are all connected to the feed port of the third material storage device; the discharge port of the third material storage device is connected to the feed port of the first gas-solid separator; the air outlet of the third material storage device is connected to the air inlet of the second dust removal device; the discharge port of the second dust removal device is connected to the feed port of the first gas-solid separator; the discharge port of the third gas-solid separator is connected to the second magnetic separation subsystem.
3. An iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 1 or 2, characterized in that: The second magnetic separation subsystem includes a slurry pool, a second grinding equipment, and a second weak magnetic separator; The discharge port of the third gas-solid separator is connected to the feed port of the slurry pool, and the discharge ports of the slurry pool, the second grinding equipment, and the second weak magnetic separator are connected to the feed port in sequence.
4. The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 2 is characterized in that: The steps include: S1 Pneumatic classification: The ore after iron ore crushing is fed into the pneumatic classification device. After the ore is processed by the pneumatic classification device, a gas phase containing fine-grained ore and a solid phase containing coarse-grained ore are obtained; the gas phase enters the fourth gas-solid separator to separate fine-grained ore and fine ore gas, the fine-grained ore is fed into the first gas-solid separator, the fine ore gas is processed by the first dust removal device, and the collected ore is fed into the first gas-solid separator, and the solid phase containing coarse-grained ore is crushed and fed into the first weak magnetic separator; S2 strong magnetic tailings discarding: the first weak magnetic separator separates the first weak magnetic concentrate and the first weak magnetic tailings; the first weak magnetic tailings are fed into the strong magnetic separator, and the strong magnetic separator separates the strong magnetic concentrate and the strong magnetic tailings; the first weak magnetic concentrate and the strong magnetic concentrate are fed into the first gas-solid separator; S3 Suspension roasting: the ore separated by the first gas-solid separator is fed into the suspension roasting device for suspension roasting, and the roasted ore is fed into the second magnetic separation subsystem; S4 Magnetic Separation after Roasting: The ore after roasting is separated into iron ore concentrate and tailings through the second magnetic separation subsystem.
5. The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 4 is characterized in that: The S3 suspension roasting comprises the following steps: The ore separated by the first gas-solid separator is fed into a suspension roasting device for suspension roasting, the roasted ore is fed into a second gas-solid separator to separate the roasted ore and roasting gas, the roasting gas is fed into the first gas-solid separator, the roasted ore is reduced in the reduction reactor and then fed into a third gas-solid separator to separate the reduced ore and the reduced gas, the reduced ore is fed into the second magnetic separator system, and the reduced gas is fed into the suspension roasting device; The gas separated by the first gas-solid separator is fed into the third material storage device to preheat the ore once. The preheated ore and the ore collected by the second dust removal device are both fed into the first gas-solid separator, and exchange heat with the roasting gas fed into the first gas-solid separator for secondary preheating and then gas-solid separation. The separated ore is fed into the suspended roasting device for roasting, and the separated gas is fed into the third material storage device to preheat the ore once.
6. The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 4 is characterized by: The classification particle size of the pneumatic classifier is 3mm; the iron grade of the iron ore is 20%-35%, the particle size is 10-20mm; the crushing particle size is 5-8mm; the crushing particle size of the coarse-grained ore is 3mm, and the content of the -200 mesh after crushing is 40%-60%; the magnetic field strength of the first weak magnetic separator is 0.1-0.3T; the magnetic field strength of the strong magnetic separator is 0.4-0.6T; The suspension roasting temperature is 600-700°C, and the ore is heated to 500-540°C during roasting.
7. The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to claim 5 is characterized by: After the first preheating, the temperature of the ore is 100-200°C, and the gas is cooled to 150-300°C; after the second preheating, the temperature of the ore is 200-300°C, and the gas is cooled to 300-400°C; the reducing gas of the reduction reaction is hydrogen or carbon monoxide, the reducing gas concentration is 20%-40%, and the reaction time is 10-30 minutes.
8. The method for using the iron ore pneumatic classification-strong magnetic tailings discarding-suspension roasting system according to any one of claims 4 to 7, characterized in that: The S4 post-calcination magnetic separation comprises the following steps: The roasted ore is ground and fed into a second weak magnetic separator for magnetic separation to obtain a second weak magnetic concentrate and a second weak magnetic tailings; the ore particle size after grinding is -200 mesh and the content is 50%-80%.