Production method of 500MPa-grade high-strength structural steel

Through the smelting-continuous casting and hot rolling process, chemical composition and temperature are controlled, and the problems of insufficient strength and elongation of high-strength steel plates in the existing technology are solved, and high-strength steel plate production that meets the automotive industry standards is achieved to meet the lightweight needs and Reduce alloy costs.

CN118932251AInactive Publication Date: 2024-11-12BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410944784.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively produce high-strength steel plates that meet the automotive lightweight needs, especially in terms of strength, elongation and surface quality, and the process performance does not fully meet the standards of the automotive industry.

Method used

The smelting-continuous casting production process is adopted, including converter smelting and LF refining, combined with hot rolling technology, and by controlling chemical composition and temperature, laminar cooling and high-pressure water phosphorus removal, we prepare 500MPa grade high-strength structural steel by controlling chemical composition and temperature, using laminar cooling and high-pressure water phosphorus removal processes.

Benefits of technology

The 500MPa grade hot rolled high-strength structural steel produced has significant strength and elongation, the surface quality and performance meet relevant standards of automobile factories, and the alloy cost is low, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932251A_ABST
    Figure CN118932251A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of 500MPa-grade high-strength structural steel. The production method is characterized by comprising the following main processes and parameters: (1) a smelting-continuous casting production process flow: molten iron pretreatment, converter treatment, LF refining and machine casting; molten steel for a casting machine comprises the following components: 0.06 to 0.08 percent of C, less than or equal to 0.2 percent of Si, 0.7 to 0.8 percent of Mn, less than or equal to 0.020 percent of P, less than or equal to 0.005 percent of S, 0.020 to 0.050 percent of Alt, 0.025 to 0.035 percent of Nb, 0.035 to 0.045 percent of Ti and the balance of Fe and inevitable impurities; (2) the tapping temperature of the converter is 1620-1640 DEG C; and (3) hot rolling production process flow. The 500MPa-grade hot-rolled high-strength structural steel disclosed by the invention has the characteristics of high strength and high ductility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical plate production, and in particular relates to a production method of 500MPa-grade high-strength structural steel. Background Art

[0002] The automobile industry has become an important pillar industry in my country's national economy. Since the beginning of the 21st century, with the rapid economic growth, the automobile industry has developed rapidly, and the amount of steel used in automobiles has continued to increase. At the same time, in order to meet the requirements of energy saving, material saving, improving the load-bearing capacity of automobiles, extending the service life and safe driving, and for the needs of environmental protection and energy saving, automobile lightweighting has become a trend in the development of the world's automobiles. Among them, high-strength steel plates play a vital role in this development process. Hot-rolled automobile structural steel QStE500TM not only has high strength, but also has good surface quality and excellent forming performance, so it is widely used in the automobile industry.

[0003] QStE500TM is a typical grade in the QStE series. It is a hot-rolled fine-grained steel for cold deformation. It is used for beam structures that require good cold forming performance and have high or high strength requirements. This material is similar to structural steel. In addition to strength requirements, it also requires a higher elongation value to ensure good processing and forming performance, and also has high requirements for surface quality, plate shape and dimensional tolerance.

[0004] QStE500TM is a low-alloy high-strength steel. The alloy design scheme adopted is to add Nb, Ti and other micro-alloying elements to low-carbon manganese steel. The chemical element Mn can eliminate or weaken the hot brittleness of steel caused by S. Nb, C and N have strong binding force, and the compounds formed can hinder the movement of austenite grain boundaries and prevent the coarsening of austenite grains during heating. At the same time, Nb can also expand the temperature range of the austenite non-recrystallization zone, increase the austenite recrystallization temperature, and thus increase the nucleation rate of ferrite. Ti is easy to form carbide Ti C with C in steel, and its dispersed precipitation can also refine the grains. Through research and exploration of controlled rolling and controlled cooling technology, reasonable industrial control of QStE420TM hot-rolled steel plates is achieved, and ultimately the comprehensive quality requirements of steel plate structure and performance are met. Summary of the invention

[0005] The purpose of the present invention is to provide a method for producing 500MPa grade high-strength structural steel. The 500MPa grade hot-rolled high-strength structural steel of the present invention has the characteristics of high strength and high elongation, and is a material widely used in automotive reinforcements and structural parts. It meets the needs of lightweight material selection for automobiles, and its mechanical properties and process properties meet the needs of relevant standards and users.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for producing 500MPa grade high-strength structural steel, comprising the following main processes and parameters:

[0008] (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-casting machine; the composition of molten steel for the casting machine is C: 0.06-0.08%, Si: ≤0.2%, Mn: 0.7-0.8%, P: ≤0.020%, S: ≤0.005%, Alt: 0.020-0.050%, Nb: 0.025-0.035%, Ti: 0.035-0.045%, and the rest is Fe and unavoidable impurities;

[0009] (2) The tapping temperature of the converter is 1620-1640℃; ensuring that the composition and temperature are coordinated;

[0010] (3) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; the ingot out-of-furnace temperature is 1220-1240℃, the rough rolling adopts 3+3 mode 2-stand rolling mill, and the initial rolling temperature of finishing rolling is 950-1030℃; the finishing rolling adopts 7-stand continuous variable crown rolling mill, and the intermediate billet thickness is 38-45mm; the final rolling temperature of finishing rolling is 880±20℃; cooling adopts laminar cooling equipment, front dispersed cooling mode, and the coiling temperature is 590±15℃.

[0011] Furthermore, the high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.10%, Mn: 0.77%, P: 0.016%, S: 0.003%, Alt: 0.029%, Nb: 0.032%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

[0012] Furthermore, the high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.12%, Mn: 0.75%, P: 0.018%, S: 0.004%, Alt: 0.027%, Nb: 0.030%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

[0013] Furthermore, the high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.10%, Mn: 0.77%, P: 0.015%, S: 0.003%, Alt: 0.035%, Nb: 0.033%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

[0014] Furthermore, the molten iron is pre-treated for desulfurization, and the molten iron is dephosphorized and decarbonized to obtain molten steel by top and bottom combined blowing converter smelting. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1630°C; the molten steel after converter smelting is then subjected to LF refining outside the furnace, the refining temperature is ≥1560°C, and the LF refining outside the furnace is performed for temperature measurement and composition fine-tuning; calcium treatment is performed after the LF treatment, and the soft blowing time is ensured to be more than 8 minutes after the calcium treatment; the overheat degree of the slab continuous casting is 25°C, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked; the slab heating temperature is 1230°C, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water; the width is fixed by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling final rolling temperature is 890°C, and the finished product thickness is 7mm; the laminar cooling adopts front dispersion cooling, the steel strip temperature is reduced to 590°C for coiling, and finally the product performance is tested.

[0015] Further, the molten iron is subjected to a desulfurization pretreatment, and the molten iron is decarbonized and dephosphorized to obtain molten steel by top and bottom combined blowing converter smelting. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1630°C; then the molten steel after converter smelting is subjected to LF refining outside the furnace, the refining temperature is ≥1560°C, and the LF refining outside the furnace is performed for temperature measurement and composition fine-tuning; the chemical composition of the LF refining casting machine is shown in Table 1, and calcium treatment is performed after the LF treatment. After the calcium treatment, the soft blowing time is ensured to be less than 8 minutes The slab continuous casting overheat is 30℃, after which the slab is cleaned, slowly cooled, and the quality of the continuous casting slab is checked; the slab heating temperature is 1235℃, the heating time is 210min, and the heated slab is dephosphorized by high-pressure water; the width is set by a fixed-width press, 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling temperature is 896℃, and the finished product thickness is 7mm; the laminar cooling adopts front dispersion cooling, the steel strip temperature is reduced to 582℃ for coiling, and finally the product performance is tested.

[0016] Further, the molten iron is subjected to a desulfurization pretreatment, and the molten iron is decarbonized and dephosphorized to obtain molten steel by top and bottom combined blowing converter smelting. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1628°C; then the molten steel after converter smelting is subjected to LF refining outside the furnace, the refining temperature is ≥1560°C, and the LF refining outside the furnace is performed for temperature measurement and composition fine-tuning; the chemical composition of the LF refining casting machine is shown in Table 1, and calcium treatment is performed after the F treatment, and the soft blowing time is ensured to be less than 8 minutes after the calcium treatment. The slab continuous casting overheat is 28℃, after which the slab is cleaned, slowly cooled, and the quality of the continuous casting slab is checked; the slab heating temperature is 1233℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water; the width is determined by a fixed-width press, 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling temperature is 896℃, and the finished product thickness is 7mm; the laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 593℃ for coiling, and finally the product performance is tested.

[0017] Compared with the prior art, the beneficial technical effects of the present invention are:

[0018] The metallographic microstructure of the 500MPa hot-rolled high-strength structural steel prepared by the present invention is mainly ferrite and contains a small amount of pearlite. The grain size is between 11 and 11.5. The 500MPa hot-rolled high-strength structural steel produced by the method provided by the present invention has been tested for use in automobile factories, and the surface quality and performance indicators have met the relevant technical standards of automobile factories and met the use requirements of relevant automobile factories. The mechanical properties and process properties meet the relevant standards and user needs. At the same time, the alloy of the present invention has low cost, simple preparation method, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings.

[0020] Figure 1 This is the microstructure diagram of Example 1 of the present invention. DETAILED DESCRIPTION

[0021] The present invention is described in more detail below through specific examples. The examples are only descriptions of the best mode of implementation of the present invention and do not limit the scope of the present invention in any way.

[0022] Example 1

[0023] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1630℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is used for temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the LF treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is guaranteed to be more than 8 minutes. . The overheat of the slab continuous casting is 25℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1230℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The finishing rolling temperature is 890℃, and the finished product thickness is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 590℃ for coiling, and finally the product performance is tested.

[0024] Example 2

[0025] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to decarbonize and dephosphorize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1630℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is subjected to temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the LF treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is ensured to be more than 8 minutes. The overheat of the slab continuous casting is 30℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1235℃, and the heating time is 210min. The heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The finishing rolling temperature is 896℃, and the finished product thickness is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 582℃ for coiling, and finally the product performance is tested.

[0026] Example 3

[0027] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to decarbonize and dephosphorize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1628℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is subjected to temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the F treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is ensured to be more than 8 minutes. The overheat of the slab continuous casting is 28℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1233℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The final rolling temperature of the finishing rolling is 896℃, and the thickness of the finished product is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 593℃ for coiling, and finally the product performance is tested.

[0028] Table 1 Chemical composition of Examples 1-3 of the present invention (wt%)

[0029]

[0030] The mechanical properties of the steel coils of Examples 1 to 3 of the present invention were tested, and the test results are shown in Table 2.

[0031] Table 2 Mechanical properties of the steel coils of Examples 1-3 of the present invention

[0032]

[0033]

[0034] It can be seen from the data in Table 2 that the mechanical properties and process properties of the 500MPa grade hot-rolled high-strength structural steel produced according to the method provided by the present invention meet the requirements of the agreement signed with the user.

[0035] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing 500MPa grade high-strength structural steel, Features: The main processes and parameters are as follows: (1) Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-casting machine; the composition of molten steel for the casting machine is C: 0.06-0.08%, Si: ≤0.2%, Mn: 0.7-0.8%, P: ≤0.020%, S: ≤0.005%, Alt: 0.020-0.050%, Nb: 0.025-0.035%, Ti: 0.035-0.045%, and the rest is Fe and unavoidable impurities; (2) The tapping temperature of the converter is 1620-1640℃; ensuring that the composition and temperature are coordinated; (3) Hot rolling production process: heating of ingot - rough rolling - finishing rolling - coiling; the ingot out-of-furnace temperature is 1220-1240℃, the rough rolling adopts 3+3 mode 2-stand rolling mill, and the initial rolling temperature of finishing rolling is 950-1030℃; the finishing rolling adopts 7-stand continuous variable crown rolling mill, and the intermediate billet thickness is 38-45mm; the final rolling temperature of finishing rolling is 880±20℃; cooling adopts laminar cooling equipment, front dispersed cooling mode, and the coiling temperature is 590±15℃.

2. The method for producing 500MPa grade high-strength structural steel according to claim 1, Features: The high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.10%, Mn: 0.77%, P: 0.016%, S: 0.003%, Alt: 0.029%, Nb: 0.032%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

3. The method for producing 500MPa grade high-strength structural steel according to claim 1, Features: The high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.12%, Mn: 0.75%, P: 0.018%, S: 0.004%, Alt: 0.027%, Nb: 0.030%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

4. The method for producing 500MPa grade high-strength structural steel according to claim 1, Features: The high-strength structural steel includes the following chemical components in mass percentage: C: 0.07%, Si: 0.10%, Mn: 0.77%, P: 0.015%, S: 0.003%, Alt: 0.035%, Nb: 0.033%, Ti: 0.036%, and the rest is Fe and unavoidable impurities.

5. The method for producing 500MPa grade high-strength structural steel according to claim 2, Features: The molten iron is pre-treated for desulfurization, and the top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1630℃; the molten steel after converter smelting is then subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃, and the LF refining outside the furnace is performed for temperature measurement and component fine-tuning; calcium treatment is performed after the LF treatment, and the soft blowing time is ensured to be more than 8 minutes after calcium treatment; the overheat of the slab continuous casting is 25℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked; the slab heating temperature is 1230℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water; the width is fixed by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling temperature is 890℃, and the finished product thickness is 7mm; the laminar cooling adopts front dispersion cooling, the steel strip temperature is reduced to 590℃ for coiling, and finally the product performance is tested.

6. The method for producing 500MPa grade high-strength structural steel according to claim 3, Features: The molten iron is subjected to desulfurization pretreatment, and the molten iron is decarbonized and dephosphorized to obtain molten steel by top and bottom combined blowing converter smelting. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1630°C; then the molten steel after converter smelting is subjected to LF refining outside the furnace, the refining temperature is ≥1560°C, and the LF refining outside the furnace is subjected to temperature measurement and composition fine-tuning; the chemical composition of the LF refining casting machine is shown in Table 1, and calcium treatment is carried out after the LF treatment, and the soft blowing time is ensured to be more than 8 minutes after the calcium treatment; The overheat degree of slab continuous casting is 30℃, after which the slab is cleaned, slowly cooled, and the quality of the continuous casting slab is checked; the slab heating temperature is 1235℃, the heating time is 210min, and the heated slab is dephosphorized by high-pressure water; the width is fixed by a fixed-width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling temperature is 896℃, and the finished product thickness is 7mm; laminar cooling adopts front dispersed cooling, and the temperature of the steel strip is reduced to 582℃ for coiling, and finally the product performance is tested.

7. The method for producing 500MPa grade high-strength structural steel according to claim 4, Features: The molten iron is subjected to desulfurization pretreatment, and the top and bottom combined blowing converter is used to decarbonize and dephosphorize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1628°C; then the molten steel after converter smelting is subjected to LF refining, the refining temperature is ≥1560°C, and the LF refining is performed for temperature measurement and composition fine-tuning; the chemical composition of the LF refining casting machine is shown in Table 1, and calcium treatment is performed after the F treatment, and the soft blowing time is guaranteed to be more than 8 minutes after the calcium treatment; the plate The overheat degree of the continuous casting billet is 28℃, after which the billet is cleaned, slowly cooled, and the quality of the continuous casting billet is checked; the billet heating temperature is 1233℃, the heating time is 205min, and the heated billet is dephosphorized by high-pressure water; the width is determined by a fixed-width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are adopted; the finishing rolling temperature is 896℃, and the finished product thickness is 7mm; laminar cooling adopts front dispersed cooling, and the temperature of the steel strip is reduced to 593℃ for coiling, and finally the product performance is tested.

Citation Information

Patent Citations

  • 500MPa-grade high-strength steel and preparation method thereof

    CN112301275A

  • Method for manufacturing 500MPa-grade seat slide rail steel based on continuous casting and rolling line

    CN112941408A

  • Production method of 460MPa-grade hot-rolled structural steel treated by rare earth

    CN118086762A

  • Production method of 450MPa grade cold rolled magnetic pole steel

    CN1904115A