Production process of rivet core line of high-tension rivet

By adopting solid solution pickling, film treatment and solid solution heat treatment steps in the production process of rivet nail core wire, the problem of scratches and insufficient tension stability of the nail core wire is solved, and a high tension and high plasticity nail core is achieved Line production to meet the sealing performance requirements of battery packs in new energy vehicles.

CN118932325APending Publication Date: 2024-11-12JIANGYIN FASTEN STAINLESS STEEL PROD CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187161.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing rivet nail core wire is prone to surface scratches and pits after processing, and the tensile strength stability is insufficient, making it difficult to meet the sealing performance requirements of high-tech requirements.

Method used

The solid solution pickling HRAP stainless steel strip is adopted, and the heat treatment and cooling rate are controlled to ensure grain grade and tension stability after film treatment, multi-pass drawing, solid solution heat treatment, single-line film treatment and inverted drawing process.

Benefits of technology

The produced nail core wire has high tension and excellent tensile stability, avoiding surface scratches and pit problems, improving sealing performance, and meeting the requirements of high tensile stress and high plasticity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a production process of a high-tension rivet core wire, which comprises the following steps: by taking a stainless steel wire rod subjected to solid solution pickling HRAP as a raw material, sequentially carrying out skin film treatment, rough drawing, solid solution heat treatment, single-wire skin film treatment and finished product drawing to obtain the rivet core wire. According to the production process of the rivet core wire, the stainless steel wire rod subjected to solid solution pickling HRAP is adopted as a raw material, single-line leather film treatment and finished product drawing are adopted, the heat treatment speed in solid solution treatment is controlled, the rivet core wire has high tension and excellent tension stability, and scratches and pits are prevented from occurring on the surface of the rivet core wire after the finished product is drawn.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal products, and in particular relates to a production process for a high-tensile-strength rivet core wire. Background Art

[0002] As the power source of new energy vehicles, the battery pack is generally located under the vehicle floor. Since the vehicle is prone to extreme conditions during operation, road water, rain, fog, dust, etc. can easily invade the battery pack, causing internal battery short circuits or even explosions. Therefore, the battery pack requires a good sealing structure to ensure good sealing performance, thereby preventing rain, fog, dust, etc. from entering the battery pack and causing damage or even danger to the battery pack. Rivets are one of the main components of the battery pack's sealing performance.

[0003] A rivet consists of a core and a shell. The core is an important component of the rivet and is made from core wire. Due to the application areas and high technical requirements of rivets, high requirements are also placed on the core wire: (1) high tensile force and good tensile stability; (2) no cracks on the surface after processing; (3) after processing, the tensile force of the nail rod with a breakpoint should be much smaller than the tensile force of the nail body; (4) low processing mold consumption. Summary of the invention

[0004] The purpose of the present invention is to provide a production process for a high-tensile-force rivet core wire, wherein the core wire produced by the process has high tensile force and excellent tensile stability, thereby avoiding scratches and pits on the surface of the core wire after the finished product is drawn.

[0005] The technical solution adopted by the present invention to solve the above problem is: a production process of a high-tensile rivet core wire, comprising the following steps: S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C≤0.03%, Mn≤2.00%, Si≤1.00%, P≤0.045%, S≤0.03%, Cr: 17.00%-19.00%, Ni: 8.00%~10.00%, Cu: 3.50%~4.00%, and the balance is Fe; S2: film treatment, immersing the stainless steel wire rod in step S1 in a film treatment tank containing a film treatment liquid, taking it out and drying it after immersion; S3: Rough drawing, the stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine for multiple passes; S4: solution heat treatment, the stainless steel wire drawn in step S3 is first pickled in an electrolytic pickling tank, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S5: single wire coating treatment, spraying the stainless steel wire after the solution heat treatment in step S4 with the coating solution, and then drying it in an oven before winding it; S6: Finished product drawing: the stainless steel wire treated with the film in step S5 is drawn to φ3.41 through an inverted wire drawing machine.

[0006] Preferably, in step S2, the film treatment liquid is TF450B film treatment liquid, the film treatment liquid concentration is 18-22wt%, the film treatment liquid temperature is 70-90°C, the immersion time is 20-30min; the drying temperature is 180-230°C, and the drying time is 90-150min; Preferably, a lubricant is used in the drawing process in step S3, and except for the last pass which uses NL305 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.), the other passes use GB205 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.).

[0007] Preferably, in step S4, the stainless steel wire in the electrolytic pickling tank serves as the anode, the lead plate serves as the cathode, and the dilute sulfuric acid solution serves as the electrolyte.

[0008] Preferably, in step S4, the solution treatment temperature is 1050-1120°C, the protective gas is N2+H2, and the heat treatment speed satisfies the wire diameter D×heat treatment speed V=10-15 (mm×m) / min, where the unit of the wire diameter is mm and the unit of the heat treatment speed is m / min.

[0009] Preferably, in step S5, the film treatment liquid is AM500 film treatment liquid, the concentration of the film treatment liquid is 10-16wt%, the temperature of the film treatment liquid is 70-90°C; the drying temperature is 300-400°C, and the drying time is 90-150min.

[0010] Preferably, a lubricant is used during the drawing process in step S6, the lubricant is AM700, the drawing reduction rate does not exceed 20%, and the drawing speed does not exceed 50 m / min.

[0011] Compared with the prior art, the advantages of the present invention are: The rivet core wire produced by the production process of the rivet core wire of the present invention has high tensile force and excellent tensile stability, wherein a direct single-wire film treatment process after annealing is adopted, which solves the problem of uneven film coating after annealing steel wire film treatment, thereby causing pits and scratches, and avoids cracks after processing; during solution heat treatment, the heat treatment production speed DV value is controlled at 10-15 (mm×m) per minute, and the cooling rate of the core wire is controlled by a water cooling tank, so that the grain grade of the core wire after solution heat treatment falls at the level of 5.0-7.0, and the strength is increased after the finished product is drawn, while maintaining high plasticity and having high tensile stress, and the comprehensive performance is excellent. DETAILED DESCRIPTION

[0012] The present invention is further described in detail below with reference to the embodiments. Example 1

[0013] A production process for a high-tensile-strength rivet core wire comprises the following steps: S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C: 0.025%, Mn: 0.61%, Si: 0.43%, P: 0.034%, S: 0.002%, Cr: 18.36%, Ni: 8.10%, Cu: 3.55%, and the balance is Fe; S2: Film treatment, immerse the φ6.5mm stainless steel wire rod selected in S1 in 80℃ film treatment liquid for 30 minutes. The film treatment liquid is TF450B aqueous solution with a concentration of 20wt%. After immersion, take it out and put it in a warm air furnace for drying. The drying temperature is 230℃ and the drying time is 100min to obtain the stainless steel wire rod after film treatment.

[0014] S3: Rough drawing. The φ6.5mm stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine in four passes. The drawing specifications of each pass are 6.5mm-5.3mm-4.5mm-4.0mm-3.7mm, and φ3.7mm stainless steel wire is obtained. Except for the last pass using NL305 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.), GB205 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used in other passes.

[0015] S4: Solution heat treatment, the stainless steel wire drawn in step S3 is first pickled in an electrolytic pickling tank (in which the stainless steel wire is used as anode, the lead plate is used as cathode, and the dilute sulfuric acid solution is used as electrolyte, and the lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing)), and then solution treated in a tubular continuous annealing furnace, the solution treatment temperature is 1100°C, the protective gas is N2+H2, the heat treatment production speed DV is controlled at 10 (mm×m) / min, and then cooled in a water cooling tank; S5: single-wire coating treatment, spraying the stainless steel wire after solution heat treatment in step S4 with coating solution, and then winding it after drying in an oven, the coating treatment liquid is AM500 coating treatment liquid, the coating treatment liquid concentration is 12wt%, the coating treatment liquid temperature is 90°C; the drying temperature is 350°C, and the drying time is 100min; S6: Finished product drawing: the stainless steel wire treated with the film in step S5 is drawn to φ3.41 mm through an inverted wire drawing machine. A lubricant is used during the drawing process. The lubricant is AM700. The drawing reduction rate is 15.06% and the drawing speed is 35 m / min.

[0016] Through the above process, a lightly drawn finished wire A with a diameter of 3.41 mm is obtained. Example 2

[0017] S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C: 0.022%, Mn: 0.63%, Si: 0.41%, P: 0.031%, S: 0.001%, Cr: 18.30%, Ni: 8.11%, Cu: 3.65%, and the balance is Fe; S2: Film treatment, immerse the φ6.5mm stainless steel wire rod selected in S1 in 80℃ film treatment liquid for 30 minutes. The film treatment liquid is TF450B aqueous solution with a concentration of 20wt%. After immersion, take it out and put it in a warm air furnace for drying. The drying temperature is 230℃ and the drying time is 100min to obtain the stainless steel wire rod after film treatment.

[0018] S3: Rough drawing. The φ6.5mm stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine in four passes. The drawing specifications of each pass are 6.5mm-5.3mm-4.5mm-4.0mm-3.73mm, and φ3.73mm stainless steel wire is obtained. Except for the last pass using NL305 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.), GB205 lubricant (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used in other passes.

[0019] S4: Solution heat treatment, the stainless steel wire drawn in step S3 is first pickled in an electrolytic pickling tank (in which the stainless steel wire is used as anode, the lead plate is used as cathode, and the dilute sulfuric acid solution is used as electrolyte, and the lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing)), and then solution treated in a tubular continuous annealing furnace, the solution treatment temperature is 1100°C, the protective gas is N2+H2, the heat treatment production speed DV is controlled at 10 (mm×m) / min, and then cooled in a water cooling tank; S5: single-wire coating treatment, spraying the stainless steel wire after solution heat treatment in step S4 with coating solution, and then winding it after drying in an oven, the coating treatment liquid is AM500 coating treatment liquid, the coating treatment liquid concentration is 12wt%, the coating treatment liquid temperature is 90°C; the drying temperature is 350°C, and the drying time is 100min; S6: Finished product drawing: the stainless steel wire treated with the film in step S5 is drawn to φ3.41 mm through an inverted wire drawing machine. A lubricant is used during the drawing process. The lubricant is AM700. The drawing reduction ratio is 16.42% and the drawing speed is 35 m / min.

[0020] Through the above process, a lightly drawn finished wire B with a diameter of 3.41 mm is obtained.

[0021] Comparative Example 1 The remaining steps are the same as those in Example 1, with the only difference being that in the S4 solid solution heat treatment step, the heat treatment production speed DV is controlled at 18 (mm×m) / min and then cooled in a water cooling tank.

[0022] Through the above process, a lightly drawn finished wire C with a diameter of 3.41 mm is obtained.

[0023] Comparative Example 2 The remaining steps are the same as those in Example 1, with the only difference being that in the S3 rough drawing step, the φ6.5mm stainless steel wire rod treated with the S2 coating is drawn in five passes through a straight-line wire drawing machine, with each drawing specification being 6.5mm-5.3mm-4.5mm-4.0mm-3.7mm-3.41mm, and the total drawing reduction rate being 72.48%, to obtain a φ3.41mm stainless steel wire, and the S6 finished product drawing step is not performed.

[0024] Through the above process, a soft finished wire D with a diameter of 3.41 mm is obtained.

[0025] Comparative Example 3 The remaining steps are the same as those in Example 1, with the only difference being that the S5 single-line coating treatment is not performed.

[0026] Through the above process, a lightly drawn finished wire E with a diameter of 3.41 mm is obtained.

[0027] The finished samples A, B, C, D, and E obtained through the above embodiments and comparative examples were tested for mechanical properties and Vickers hardness according to GB / T 228.1 and GB / T4340.1, and the results are shown in Table 1 below.

[0028] Table 1 Performance test results of nail core wires of Examples 1-2 and Comparative Examples 1-3

[0029] It can be seen from the above table that compared with conventional production processes, the 3.41mm nail core wire produced by the present invention has higher strength while ensuring a higher elongation after break. The hardness difference between the inside and outside of the nail core wire is obvious, and the comprehensive performance is excellent. It can meet customers' requirements for high tensile stress and high plasticity. From the above results, the total amount of rough drawing deformation is controlled not to exceed 70%, and the heat treatment production speed DV value is controlled at 10 (mm×m) per minute during solution heat treatment. The cooling rate of the nail core wire is controlled by a water cooling tank, so that the grain grade of the nail core wire after solution heat treatment falls at the level of 5.0 to 7.0. The single-wire film process ensures the surface quality of the finished product during drawing. After the finished product is drawn, the strength increases, and it has high tensile stress while maintaining high plasticity, and the comprehensive performance is excellent.

[0030] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A production process for high-tensile rivet core wire, characterized in that: Includes the following step: S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C≤0.03%, Mn≤2.00%, Si≤1.00%, P≤0.045%, S≤0.03%, Cr: 17.00%-19.00%, Ni: 8.00%~10.00%, Cu: 3.50%~4.00%, and the balance is Fe; S2: film treatment, immersing the stainless steel wire rod in step S1 in a film treatment tank containing a film treatment liquid, taking it out and drying it after immersion; S3: Rough drawing, the stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine for multiple passes; S4: solution heat treatment, the stainless steel wire drawn in step S3 is first pickled in an electrolytic pickling tank, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S5: single wire coating treatment, spraying the stainless steel wire after the solution heat treatment in step S4 with the coating solution, and then drying it in an oven before winding it; S6: Finished product drawing, the stainless steel wire treated with the film in step S5 is drawn through an inverted wire drawing machine.

2. The production process of high-tensile rivet core wire according to claim 1, characterized in that: In step S2, the film treatment liquid is TF450B film treatment liquid, the film treatment liquid concentration is 18~22wt%, the film treatment liquid temperature is 70~90℃, the immersion time is 20~30min; the drying temperature is 180~230℃, and the drying time is 90~150min.

3. The production process of high-tensile rivet core wire according to claim 1, characterized in that: Lubricant is used in the drawing process in step S3.

4. The production process of high-tensile rivet core wire according to claim 1, characterized in that: In step S4, the stainless steel wire in the electrolytic pickling tank is used as the anode, the lead plate is used as the cathode, and the dilute sulfuric acid solution is used as the electrolyte.

5. The production process of high-tensile rivet core wire according to claim 1, characterized in that: In step S4, the solution treatment temperature is 1050~1120°C, the protective gas is N2+H2, and the heat treatment speed satisfies the wire diameter D×heat treatment speed V=10~15 (mm×m) / min, where the unit of the wire diameter is mm and the unit of the heat treatment speed is m / min.

6. The production process of high-tensile rivet core wire according to claim 1, characterized in that: In step S5, the film treatment liquid is AM500 film treatment liquid, the concentration of the film treatment liquid is 10-16wt%, the temperature of the film treatment liquid is 70-90°C; the drying temperature is 300-400°C, and the drying time is 90-150min.

7. The production process of high-tensile rivet core wire according to claim 1, characterized in that: During the drawing process in step S6, a lubricant is used, the lubricant is AM700, the drawing reduction rate does not exceed 20%, and the drawing speed does not exceed 50 m / min.