High-entropy alloy coating and in-situ generation preparation method thereof

Through cold spraying and friction stir treatment technology, high-entropy alloy coatings with high binding strength and high plasticity are formed on the surface of flexible metal substrates such as magnesium alloy, aluminum alloy and copper alloy, which solves the difficulty of coating formation and binding force in the prior art. The problem of insufficient results has achieved high-quality surface modification.

CN118932328APending Publication Date: 2024-11-12CHINA WEAPON SCI ACADEMY NINGBO BRANCH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411015290.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Prior Art When preparing high-entropy alloy coatings on flexible metal substrate surfaces such as magnesium alloys, aluminum alloys and copper alloys, there is difficulty in forming an effective coating due to laser cladding, low thermal spray bonding strength, and high matrix temperature during PVD, resulting in coating. The problem of difficulty in preparing the layer.

Method used

The first high-entropy alloy coating is formed on the surface of the substrate by cold spraying technology, and the first high-entropy alloy coating is alloyed with the selected metal material through friction stir treatment to form the second high-entropy alloy coating, which improves the bonding strength and plasticity, and reduces the coating and Temperature gradient of the substrate.

Benefits of technology

It significantly improves the bonding strength and plasticity of high-entropy alloy coatings, solves the problems of coating brittleness and bonding strength, and realizes a high-quality surface coating, suitable for matrixes such as aluminum alloys, magnesium alloys and copper alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932328A_ABST
    Figure CN118932328A_ABST
Patent Text Reader

Abstract

The invention discloses a high-entropy alloy coating and an in-situ generation preparation method thereof. The preparation method comprises the steps that a first high-entropy alloy coating is formed on the surface of a base body, and the base body is made of a selected metal material; and friction stir treatment is conducted through the first high-entropy alloy coating, and after the first high-entropy alloy coating and selected metal are alloyed, a second high-entropy alloy coating is formed. According to the preparation method provided by the invention, the first high-entropy alloy is firstly formed on the surface of the substrate as the coating, and then the selected metal material at the interface of the substrate and the first high-entropy alloy are alloyed by utilizing the stirring friction treatment with controllable action depth, so that the bonding state of deposited particles is improved, grains can be refined, and the performance of the coating is improved. And meanwhile, the temperature gradient of the coating and a matrix is also remarkably reduced in the treatment process, so that the thermal stress can be effectively reduced, the initiation of cracks in the coating is prevented, a high-quality surface coating is finally obtained, and the problems of brittleness and binding force faced by a cold spraying coating are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface processing and modification, and in particular to a high entropy alloy coating and an in-situ generation preparation method thereof. Background Art

[0002] High entropy alloy (HEA) is a new type of metal material composed of multiple main elements. Due to the lattice distortion effect caused by the multi-principal element composition, high entropy alloy has higher strength and hardness. The hysteresis diffusion effect makes high entropy alloy have a more stable phase structure and thermodynamic properties, showing excellent high temperature performance, corrosion resistance and wear resistance. Introducing high entropy alloy coatings on various substrate surfaces can achieve various functions.

[0003] At present, the main processes for preparing high entropy alloy coatings include thermal spraying, plasma cladding, laser cladding and physical vapor deposition. For example, the Chinese invention patent with publication number CN 117070934 B discloses the use of multi-layer laser cladding to prepare high entropy alloys; the Chinese invention patent with publication number CN 117488140 A discloses the use of supersonic flame spraying + vacuum heat treatment to prepare a high corrosion-resistant and high wear-resistant NiCrCoBSi high entropy alloy coating on the surface of CrZrCu alloy; and the Chinese invention patent with publication number CN 113966408B discloses the use of physical vapor deposition technology to prepare a nitrogen oxide high entropy alloy coating.

[0004] Although the above methods can all prepare high entropy alloy coatings, there are the following problems when strengthening the surfaces of relatively flexible metal substrates such as magnesium alloys, aluminum alloys and copper alloys: 1) Due to the high thermal conductivity and reflectivity of aluminum alloys and copper alloys, it is difficult for laser cladding technology to form an effective coating on the alloy surface; 2) The bonding strength between thermal spray coatings and magnesium alloy, aluminum alloy and copper alloy substrates is low; 3) During the PVD process, the substrate temperature is relatively high, making it difficult to prepare coatings on the surfaces of low-melting-point metals such as aluminum alloys and magnesium alloys.

[0005] In order to solve the above problems, cold spray technology has been developed in this field, which provides an important process method for high-performance coatings. Its characteristics are that it has little effect on the organizational structure of the material and has a very high powder particle deposition efficiency. However, due to the high brittleness of the cold sprayed coating and the low bonding strength, its application is limited to a certain extent. Summary of the invention

[0006] In view of the deficiencies in the prior art, an object of the present invention is to provide a high entropy alloy coating and a method for preparing the same by in-situ generation.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0008] In a first aspect, the present invention provides a method for preparing an in-situ high-entropy alloy coating with high bonding strength and high plasticity, comprising:

[0009] Forming a first high entropy alloy coating on the surface of the substrate, wherein the contact portion between the substrate and the first high entropy alloy coating is made of a selected metal material;

[0010] A friction stir treatment is performed through the first high entropy alloy coating, and the action depth of the friction stir treatment is greater than the thickness of the high entropy alloy coating, so that the first high entropy alloy coating is alloyed with the selected metal to form a second high entropy alloy coating.

[0011] In a second aspect, the present invention further provides a high entropy alloy coating obtained by the above-mentioned preparation method, wherein the high entropy alloy coating is formed on the surface of a substrate, and the high entropy alloy coating is formed by alloying a selected metal material on the surface of the substrate with an initial high entropy alloy component;

[0012] Furthermore, the high entropy alloy coating includes an original layer and a transition layer, the transition layer is located between the substrate and the original layer, the high entropy alloy in the transition layer is a second high entropy alloy coating formed by alloying the first high entropy alloy coating with the selected metal material, and the original coating still maintains the material of the first high entropy alloy coating.

[0013] Based on the above technical solution, compared with the prior art, the beneficial effects of the present invention at least include:

[0014] The preparation method provided by the present invention first forms a first high entropy alloy as a coating on the surface of a substrate, and then uses a stir friction treatment with controllable action depth to alloy the selected metal material at the interface of the substrate with the first high entropy alloy, thereby improving the bonding state of the deposited particles, refining the grains, and significantly improving the plasticity of the coating. At the same time, the temperature gradient between the coating and the substrate is also significantly reduced during the treatment process, thereby effectively reducing thermal stress and preventing the initiation of cracks inside the coating, ultimately obtaining a high-quality surface coating, and solving the brittleness and bonding problems faced by cold spray coatings.

[0015] The above description is only an overview of the technical solution of the present invention. In order to enable those skilled in the art to more clearly understand the technical means of the present application and implement them according to the contents of the specification, the following is a description of the preferred embodiments of the present invention in conjunction with detailed drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the preparation state of the preparation method provided by a typical implementation case of the present invention;

[0017] Figure 2It is a schematic structural diagram of a stirring head used in a preparation method provided in a typical embodiment of the present invention;

[0018] Figure 3 This is an EBSD inverse polarity image of a high entropy alloy coating prepared in a typical implementation case of the present invention;

[0019] Figure 4 It is a surface electron microscope image of an alloy coating prepared in a typical comparative example of the present invention.

[0020] Explanation of the accompanying drawings: 1. Stirring head; 11. Cooling channel; 2. First high entropy alloy coating; 3. Substrate; 4. Temperature control device. DETAILED DESCRIPTION

[0021] In view of the deficiencies in the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution, its implementation process and principle will be further explained as follows.

[0022] The purpose of the present invention is to provide a method for preparing an in-situ generated high entropy alloy coating on the surface of a substrate A, so as to achieve lightweight materials and have excellent mechanical properties. The in-situ generated high entropy alloy C obtained by cold spraying a high entropy alloy layer B in the early stage and subsequent treatment has high density and good dispersibility, and it can be independent of complex processes and does not cause pollution.

[0023] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0024] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component or method step from another with the same name, but do not necessarily require or imply any such actual relationship or order between these components or method steps.

[0025] See also Figure 1 As shown, an embodiment of the present invention provides a method for preparing an in-situ high-entropy alloy coating with high bonding strength and high plasticity, which comprises the following steps:

[0026] A first high entropy alloy coating 2 is formed on the surface of the substrate 3 by cold spraying, and the contact portion between the substrate 3 and the first high entropy alloy coating 2 is made of a selected metal material.

[0027] The surface of the first high entropy alloy coating 2 is subjected to a friction stir treatment, and the action depth of the friction stir treatment is greater than the thickness of the high entropy alloy coating, so that the first high entropy alloy coating 2 is alloyed with the selected metal to form a second high entropy alloy coating.

[0028] As some typical examples of the above technical solutions, the specific preparation process includes, for example:

[0029] 1) Degrease, dry and polish the surface of substrate A.

[0030] 2) The high entropy alloy powder B for spraying is loaded into a cold spraying powder feeding tank, and a cold spraying device controlled by a robotic arm is used to obtain a composite component after cold spraying a high entropy alloy layer B of a certain thickness on the substrate A treated in the step 1), and the surface of the high entropy alloy layer B of the composite component is mechanically processed to obtain a composite component with a smooth surface and a B thickness of h1.

[0031] 3) The surface of the high entropy alloy layer B of the composite component in step 2) is subjected to a stir friction treatment, with a stirring depth of h2.

[0032] 4) In step 3), the X atoms in the composite component matrix A and the atoms in the high entropy alloy layer B undergo a chemical reaction during the stirring friction process, and finally an in-situ generated high entropy alloy C coating is obtained on the surface of the matrix A.

[0033] The above technical solution is a preparation method for in-situ generating a high-entropy alloy coating with high bonding strength and high plasticity, that is, firstly cold spraying is performed on a low-melting-point substrate 3 to form a first high-entropy alloy, and then a stir friction treatment is used to make the first high-entropy alloy and the X metal element of the substrate 3 diffuse with each other to form a new second high-entropy alloy.

[0034] The inventors of the present invention believe that the advantages of preferably using a cold spraying film-forming method in combination with stir friction are at least that: cold spraying prevents the first high entropy alloy coating 2 from being oxidized, and can maintain the original powder state characteristics, providing a basis for the subsequent stir friction to prepare a new type of high entropy alloy; the coating particles are directly combined as a mechanical bond, and the interface has a "loose" channel, which is conducive to the diffusion of the X element, so that the distribution of the X element after stir friction is more uniform, and no segregation will be formed.

[0035] In some embodiments, the second high entropy alloy coating has stronger physical and chemical properties than the first high entropy alloy coating 2.

[0036] In some embodiments, the physical and chemical properties include any one or a combination of two or more of bonding strength, hardness, toughness, and corrosion resistance.

[0037] Some existing technologies provide a technical solution for plasma spraying a high entropy alloy layer on the surface of a copper or similar metal substrate 3, and then using stir friction to form a surface composite coating. However, due to differences in technical ideas and specific implementation processes, what is formed is still a composite film layer with the substrate 3 material as the main material and the high entropy alloy embedded in the main layer, but essentially no alloying is formed, and the high entropy alloy is distributed in a regionalized point-like manner in the composite coating.

[0038] The technical concept of the present invention is different from this. By controlling the degree of stirring of the selected metal material at the interface between the first high entropy alloy layer and the substrate 3, what is formed is not a regionalized inlaid film layer structure, but a fully alloyed high entropy alloy integrated film layer. The main effect is that the bonding strength and plasticity of the film layer are significantly improved compared with the first high entropy alloy coating 2, rather than compared with the substrate 3 itself.

[0039] In addition, due to the different formation methods of the first high entropy alloy coating 2, the present invention is also essentially different from the previous prior art:

[0040] In terms of the problem to be solved, the present invention solves the problem of bonding strength and brittleness of the first high entropy alloy coating 2 formed by cold spraying, while the coating formed by plasma spraying does not face this problem.

[0041] In terms of specific microscopic behavior, since the first high entropy alloy coating 2 formed by plasma spraying is a dense layer of metallurgical bonding coating with strong intra-layer bonding, even if a controlled stirring friction treatment is applied, it is not enough to form an alloyed second high entropy alloy coating, but will still form a microscopically separated physical bonding structure. At the same time, the plasma sprayed coating is very easy to form a stable oxide, and a new type of high entropy alloy coating cannot be formed in the subsequent stirring friction process. However, in the present invention, the coating obtained by cold spraying is fully utilized to be more "loose" than plasma spraying, so that the substrate 3 metal and the coating material can fully diffuse and fuse under the action of stirring friction, and finally form an alloyed integrated film layer. This is a phenomenon that cannot be achieved by adjusting the stirring friction conditions in the comparative document 1.

[0042] As for the specific material selection, in some embodiments, the first high entropy alloy coating 2 does not contain any metal element of the selected metal material.

[0043] In some embodiments, the material of the first high entropy alloy coating 2 includes a high entropy alloy composed of any three or more metal elements of Fe, Co, Cr, Ni, Ta, Mo, Nb, W, V, Al, Cu, and Ti. For example, it can be a three-principal element high entropy alloy, or it can be a four-principal element, five-principal element, or multi-principal element high entropy alloy.

[0044] In some embodiments, the selected metal includes any one of Al, Mg, Cr, Zr, Cu, and Ti, or an alloy formed by the single metal and a non-metal, or an alloy formed by a combination of two or more thereof and a non-metal element that may be added or not added.

[0045] In addition, in some embodiments, the preparation method may specifically include the following pre-treatment steps:

[0046] Before the cold spraying is performed, the substrate 3 is subjected to surface finishing, and the surface finishing at least includes polishing the surface of the substrate 3 .

[0047] In some embodiments, the formation process of the first high entropy alloy specifically includes:

[0048] The original high entropy alloy coating was formed by cold spraying process.

[0049] The original high entropy alloy coating is mechanically processed to reduce the thickness of the original high entropy alloy coating and improve the surface smoothness, thereby obtaining the first high entropy alloy coating 2.

[0050] In a preferred embodiment of the present invention, spraying is first performed to form an original coating, and then the original coating is mechanically processed (such as polishing or grinding, etc.) to thin the original coating, thereby obtaining an implementation method of the first high entropy alloy coating 2. This is because the surface of the cold sprayed state is rough and the particles are relatively loose. Directly stirring and rubbing after spraying will cause the new coating to be unable to form and will cause a large number of defects such as holes and cracks. The purpose of mechanical processing is to make the coating surface smooth to facilitate subsequent stirring and friction treatment.

[0051] Regarding specific implementation conditions, in some embodiments, if the thickness of the first high entropy alloy coating 2 is defined as h1 and the action depth is defined as h2, then:

[0052] h1 <h2≤5h1。

[0053] In some embodiments, in general, the value range of h1 is 30-100 μm. Generally, for thinner coatings, a complete second high entropy alloy coating can be obtained by stir friction treatment, while for thick coatings (e.g., a thickness of more than 100 μm, but the thickness may vary depending on the coating material and process conditions), the second high entropy alloy coating may only exist at the interface between the coating and the substrate (that is, the transition layer described in some embodiments below). Both of these thickness coatings can form a second high entropy alloy coating, but there are some differences in the specific structure of the coating.

[0054] In some embodiments, the friction stir process is carried out at a speed of 10 to 50 mm / min, and the temperature at the stirring center is maintained at 300 to 800° C. The ultimate purpose of other conditions in the friction stir process, such as the rotation speed and the diameter of the stirring head, is to obtain a reasonable temperature at the stirring center to allow the X element to diffuse. Therefore, maintaining the temperature is the core parameter, and other parameters are mostly adaptively adjusted for this purpose, which can be obtained through conditional tests.

[0055] In a representative embodiment, the stirring tool travels at a speed of 10 mm / min to 50 mm / min during the friction stirring treatment, the temperature at the stirring center is maintained at 300 to 800° C., and the friction stirring depth h1 <h2≤Sh1。

[0056] In the above preferred embodiment, the parameters of the travel speed, stirring depth and stirring center temperature are very important. The inventors have found in practice that the travel speed, stirring depth and stirring center temperature determine the diffusion degree and diffusion speed of the X metal of the matrix 3 and the first high entropy alloy. For example, if the travel speed is too fast, the heat input will be low, the temperature of the stirring center will be low, the fluidity of the metal will be poor, the stirring zone will easily produce defects, and the diffusion speed of the X metal of the matrix 3 and the first high entropy alloy will be slow, and the second high entropy alloy cannot be formed; if the travel speed is too slow, the heat input will be high, the temperature of the stirring center will be high, and the fluidity of the metal will be strong, so that part of the plastic metal will overflow to form flash, resulting in the lack of metal inside the stirring zone, forming holes, and at the same time, the high temperature will lead to coarse grains, reducing the performance of the second high entropy alloy. If the stirring depth is too high, the matrix 3 may be stirred too much, and the X metal element of the matrix 3 will be introduced into the first high entropy alloy too much, reducing the performance of the second high entropy alloy; if the stirring depth is too low, the X metal element of the matrix 3 will be introduced into the first high entropy alloy too little, and the desired second high entropy alloy performance cannot be formed. Therefore, in order to successfully achieve the in-situ generation of the second high entropy alloy, good condition control is more important.

[0057] In some embodiments, a cooling channel 11 is provided inside the stirring head 1 used for the friction stir treatment, and the cooling channel 11 is continuously utilized to cool the liquid cooling medium during the friction stir treatment.

[0058] In some embodiments, the stirring head 1 is in the shape of a rectangle, a triangle or a trapezoid.

[0059] In some embodiments, the substrate 3 is supported on a temperature control device 4 , and the substrate 3 is continuously cooled by the temperature control device 4 during the friction stir treatment.

[0060] As a specific example, the stirring head 1 during the stir friction treatment is made of tungsten-rhenium alloy or tungsten-steel alloy, and the stirring head 1 is designed with a water cooling channel inside to cool the stirring head 1. The shape of the stirring head 1 is any one of a rectangle, a triangle or a trapezoid.

[0061] The significant advantages of the above preparation method are:

[0062] 1. The coating and the substrate 3 are metallurgically bonded with high bonding strength. Various high entropy alloys can be prepared on the surface of aluminum alloys, magnesium alloys and copper alloys to achieve excellent bonding between the coating and the substrate 3.

[0063] 2. As a solid coating preparation technology, the present invention reduces the temperature gradient between the coating and the substrate 3, thereby effectively reducing thermal stress and preventing the initiation of cracks inside the coating.

[0064] 3. The coating has high plasticity. The cold sprayed coating is very brittle. The friction stir treatment improves the bonding state of the deposited particles, refines the grains, and significantly improves the plasticity of the coating.

[0065] 4. The process is simple, efficient and low-cost, and can be used to prepare various primary high-entropy alloy coatings.

[0066] On the other hand, an embodiment of the present invention also provides a high-entropy alloy coating obtained by the preparation method provided in any of the above-mentioned embodiments, wherein the high-entropy alloy coating is formed on the surface of the substrate 3, and the high-entropy alloy coating is formed by alloying the selected metal material on the surface of the substrate 3 with the initial high-entropy alloy component.

[0067] Regarding more specific structural features, in some embodiments, corresponding to the different situations shown above, when a thicker first high entropy alloy coating is used, the high entropy alloy coating includes an original layer and a transition layer, and the transition layer is located between the substrate and the original layer. The high entropy alloy in the transition layer is a second high entropy alloy coating formed by alloying the first high entropy alloy coating with the selected metal material, and the original coating still maintains the material of the first high entropy alloy coating.

[0068] The technical solution of the present invention is further described in detail below through several embodiments and in conjunction with the accompanying drawings. However, the selected embodiments are only used to illustrate the present invention, and do not limit the scope of the present invention.

[0069] Example 1

[0070] A method for preparing an in-situ high entropy alloy coating on the surface of a substrate A comprises the following steps:

[0071] 1) The substrate A is made of 6061 aluminum alloy, and the surface of the plate-shaped aluminum alloy substrate with a size of 120mm×90mm×40mm is degreased, dried and polished. Because aluminum alloy has good thermal conductivity and heat dissipation, it can keep the internal temperature uniform during the cold spraying process, and it is convenient to control the temperature within a certain range to reduce deformation, cracking and other problems caused by temperature concentration.

[0072] 2) The high entropy alloy (FeCoCrNi) powder B for spraying is loaded into a cold spraying powder feeding tank, and a cold spraying device controlled by a robotic arm is used to additively manufacture a high entropy alloy layer B on the aluminum alloy substrate treated in step 1) to obtain a composite component. The thickness of the high entropy alloy layer increases with the number of spraying passes, and the size of the high entropy alloy layer B gradually increases in the three-dimensional direction until a high entropy alloy layer with a thickness greater than or equal to 150 μm is obtained.

[0073] 3) The composite component in step 2) is subjected to cutting mechanical processing (such as wire cutting and abrasive flow inner hole polishing) until the thickness of the high entropy alloy layer B in the composite component is 50 μm.

[0074] 4) The high entropy alloy layer B in the composite component obtained in step 3) is subjected to a friction stir treatment. The material of the stirring head is tungsten steel alloy, and the shape is selected as a trapezoid. There is a water cooling system inside the stirring head to prevent the strength of the stirring head from being reduced at high temperatures. During the stirring process, the temperature of the stirring center is controlled at 300°C and the stirring depth is 300μm.

[0075] The high entropy alloy C (FeCoCrNiAl) coating is generated in situ on the aluminum alloy surface by friction stir treatment, so that the material has good mechanical properties while being lightweight. Table 1 shows the data of hardness, bending strength and fracture toughness of the high entropy alloy C (FeCoCrNiAl) coating. The EBSD reverse polarity image of the high entropy alloy coating prepared in this embodiment is shown in Figure 1. Figure 3 As shown, the typical high entropy alloy structure can be clearly seen.

[0076] Table 1 Coating hardness, bending strength and fracture toughness

[0077] Sample Hardness (HV0.3) Bending strength(MPa) <![CDATA[Fracture toughness (Mpa·m 1 / 2 )]]> 1 380 540 61 2 385 515 58 3 373 530 55

[0078] Comparative Example 1

[0079] This comparative example is substantially the same as Example 1, except that:

[0080] Step (2) uses plasma spraying to form a high entropy alloy layer with the same composition, and the remaining steps are exactly the same as in Example 1.

[0081] SEM analysis of the coating shows that Figure 4In the image shown, no large amount of alloy phase is observed, but rather dispersed physical bonds, with particles embedded within the Al alloy matrix without forming an integral alloy.

[0082] This shows that the key to the in-situ formation of the second high-entropy metal alloy coating is to combine cold spraying with friction stir processing and use the characteristics of the organizational structure brought by cold spraying for alloying.

[0083] Comparative Example 3

[0084] This comparative example is substantially the same as Example 1, except that:

[0085] In step (4), the stirring depth is increased to 1 mm.

[0086] The surface film layer obtained in this comparative example is similar to some prior arts, and forms a structure in which a large amount of aluminum alloy serves as the main body of the film layer, and a small amount of the first high entropy alloy serves as particles embedded in the main layer. The performance of this structure in terms of hardness, wear resistance and bonding strength is significantly weaker than that of the fully alloyed integral second high entropy alloy layer formed in Example 1.

[0087] Table 2 shows the data of hardness, bending strength and fracture toughness of high entropy alloy coating.

[0088] Table 2 Coating hardness, bending strength and fracture toughness

[0089]

[0090]

[0091] Example 2

[0092] A method for preparing an in-situ high entropy alloy coating on the surface of a substrate A comprises the following steps:

[0093] 1) The substrate A is made of CrZrCu alloy, and the surface of the plate-shaped copper alloy substrate with a size of 120 mm × 90 mm × 40 mm is degreased, dried and polished.

[0094] 2) The high entropy alloy (FeCoCrNi) powder B for spraying is loaded into a cold spray powder feeding tank, and a cold spraying device controlled by a robotic arm is used to additively manufacture a high entropy alloy layer B on the copper alloy substrate treated in step 1) to obtain a composite component. The thickness of the high entropy alloy layer increases with the number of spraying passes, and the size of the high entropy alloy layer B gradually increases in the three-dimensional direction until a high entropy alloy layer with a thickness greater than or equal to 150 μm is obtained.

[0095] 3) The composite component in step 2) is subjected to cutting and mechanical processing until the thickness of the high entropy alloy layer B in the composite component is 50 μm.

[0096] 4) The high entropy alloy layer B in the composite component obtained in step 3) is subjected to a friction stir treatment. The material of the stirring head is tungsten steel alloy, and the shape is selected to be trapezoidal. There is a water cooling system inside the stirring head to prevent the strength of the stirring head from being reduced at high temperatures. During the stirring process, the temperature of the stirring center is controlled at 700°C and the stirring depth is 55μm.

[0097] After friction stir treatment, a high entropy alloy C (FeCoCrNiCu) coating is generated in situ on the surface of the copper alloy.

[0098] Tables 3 and 4 give the data of hardness, bending strength and conductivity of high entropy alloy B and high entropy alloy C coatings respectively.

[0099] Table 3 Hardness, bending strength and conductivity of high entropy coating B

[0100] Sample Hardness (HV0.3) Bending strength(MPa) <![CDATA[Conductivity (10 -5 Ω·m)]]> 1 351 502 9.8 2 329 527 8.4 3 346 532 8.7

[0101] Table 4 Hardness, bending strength and conductivity of high entropy coating C

[0102]

[0103]

[0104] Example 3

[0105] A method for preparing an in-situ high entropy alloy coating on the surface of a substrate A comprises the following steps:

[0106] 1) The substrate A is made of TC4 titanium alloy, and the surface of the plate-shaped titanium alloy substrate with a size of 120 mm × 90 mm × 40 mm is degreased, dried and polished.

[0107] 2) The high entropy alloy (FeCoCrNi) powder B for spraying is loaded into a cold spraying powder feeding tank, and a cold spraying device controlled by a robotic arm is used to additively manufacture a high entropy alloy layer B on the titanium alloy substrate treated in step 1) to obtain a composite component. The thickness of the high entropy alloy layer increases with the number of spraying passes, and the size of the high entropy alloy layer B gradually increases in the three-dimensional direction until a high entropy alloy layer with a thickness greater than or equal to 150 μm is obtained.

[0108] 3) The composite component in step 2) is subjected to cutting and mechanical processing until the thickness of the high entropy alloy layer B in the composite component is 50 μm.

[0109] 4) The high entropy alloy layer B in the composite component obtained in step 3) is subjected to a friction stir treatment. The material of the stirring head is tungsten steel alloy, and the shape is selected to be trapezoidal. There is a water cooling system inside the stirring head to prevent the strength of the stirring head from being reduced at high temperatures. During the stirring process, the temperature of the stirring center is controlled at 800°C and the stirring depth is 180μm.

[0110] After friction stir treatment, a high entropy alloy C (FeCoCrNiTi) coating is generated in situ on the surface of the titanium alloy.

[0111] Tables 5 and 6 give the data of hardness, bending strength and corrosion performance of high entropy alloy B and high entropy alloy C coatings in 1M H2SO4 solution.

[0112] Table 5 Hardness, bending strength and corrosion properties of high entropy alloy B coating

[0113] Sample Hardness (HV0.3) Bending strength(MPa) Corrosion potential (mV) <![CDATA[Corrosion current (10 -6 A / cm 2 )]]> 1 351 502 -1182 8.8 2 329 527 -1226 7.6 3 346 532 -1217 8.4

[0114] Table 6 Hardness, bending strength and corrosion properties of high entropy alloy C coating

[0115]

[0116]

[0117] Based on the above embodiments and comparative examples, it can be clearly seen that the preparation method provided in the embodiments of the present invention first forms a first high entropy alloy as a coating on the surface of the substrate, and then utilizes a stir friction treatment with controllable action depth to alloy the selected metal material at the interface of the substrate with the first high entropy alloy, thereby improving the bonding state of the deposited particles, refining the grains, and significantly improving the plasticity of the coating. At the same time, the temperature gradient between the coating and the substrate is also significantly reduced during the treatment process, thereby effectively reducing thermal stress and preventing the initiation of cracks inside the coating, ultimately obtaining a high-quality surface coating, and solving the brittleness and bonding problems faced by cold spray coatings.

[0118] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an in-situ high-entropy alloy coating with high bonding strength and high plasticity, characterized in that: include: A first high entropy alloy coating is formed on the surface of the substrate by cold spraying, and the contact portion between the substrate and the first high entropy alloy coating is made of a selected metal material; A friction stir treatment is performed through the first high entropy alloy coating, and the action depth of the friction stir treatment is greater than the thickness of the high entropy alloy coating, so that the first high entropy alloy coating is alloyed with the selected metal to form a second high entropy alloy coating.

2. The preparation method according to claim 1, characterized in that: The second high entropy alloy coating has stronger physical and chemical properties than the first high entropy alloy coating; Preferably, the physical and chemical properties include any one or a combination of two or more of bonding strength, hardness, toughness, and corrosion resistance.

3. The preparation method according to claim 1, characterized in that: The first high entropy alloy coating does not contain any metal element in the selected metal material.

4. The preparation method according to claim 1 or 3, characterized in that: The material of the first high entropy alloy coating includes a high entropy alloy composed of any three or more metal elements of Fe, Co, Cr, Ni, Mn, Ta, Mo, Nb, W, V, Al, Cu, and Ti; And / or, the selected metal includes any one metal element among Al, Mg, Cr, Zr, Cu, Ti or an alloy formed by the element and a non-metal, or an alloy formed by a combination of two or more thereof and a non-metal element which may be added or not added.

5. The preparation method according to claim 1, characterized in that: Specifically include: Before the cold spraying is performed, the substrate is subjected to surface finishing, and the surface finishing at least includes polishing the surface of the substrate.

6. The preparation method according to claim 1, characterized in that: The formation process of the first high entropy alloy specifically includes: The original high entropy alloy coating is formed by cold spraying process; The original high entropy alloy coating is mechanically processed to reduce the thickness of the original high entropy alloy coating and improve the surface smoothness, thereby obtaining the first high entropy alloy coating.

7. The preparation method according to claim 1, characterized in that: If the thickness of the first high entropy alloy coating is defined as h1, and the action depth is defined as h2, then: h1 <h2≤5h1。 8. The preparation method according to claim 1, characterized in that: The friction stir treatment is carried out at a speed of 10 to 50 mm / min, and the temperature of the stirring center is maintained at 300 to 800°C.

9. The preparation method according to claim 1 or 8, characterized in that: A cooling channel is provided inside the stirring head used for the friction stir treatment, and the cooling channel is continuously used to cool the liquid cooling medium during the friction stir treatment; And / or, the stirring head is in any one of a rectangular, triangular or trapezoidal shape; And / or, the substrate is supported on a temperature control device, and the substrate is continuously cooled by the temperature control device during the friction stir treatment.

10. A high entropy alloy coating obtained by the preparation method according to any one of claims 1 to 9, wherein the high entropy alloy coating is formed on the surface of a substrate, characterized in that: The high entropy alloy coating is formed by alloying the selected metal material on the surface of the substrate with the initial high entropy alloy component; Preferably, the high entropy alloy coating includes an original layer and a transition layer, the transition layer is located between the substrate and the original layer, the high entropy alloy in the transition layer is a second high entropy alloy coating formed by alloying the first high entropy alloy coating with the selected metal material, and the original coating still maintains the material of the first high entropy alloy coating.

Citation Information

Cited By

  • Preparation method of high-entropy alloy gradient coating based on layer-by-layer solid phase densification

    CN121976144A

  • A method for preparing high-entropy alloy gradient coatings based on layer-by-layer solid-phase densification