MgLiAlCe-LDHs (at) GO-5NH3 film as well as preparation method and application thereof
Through the preparation of the quaternary MgLiAlCe-LDHs@GO-5NH3 film layer, graphene oxide and corrosion inhibitors are used to extend the diffusion path of corrosive media and form a self-healing barrier, which solves the problem of poor corrosion resistance of magnesium lithium alloys and achieves efficient Corrosion resistance and self-repair performance, suitable for the aerospace and automotive industries.
Patent Information
- Application Number
- CN202410984432.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Magnesium lithium alloy has poor corrosion resistance, and the existing LDHs film layer structure is loose, which cannot effectively block the corrosion environment, resulting in the failure of the film layer.
The preparation method of the quaternary MgLiAlCe-LDHs@GO-5NH3 film layer was adopted, and a dense film layer was formed by microarc oxidation, cerium salt sealing, in situ growth and anion exchange method, and graphene oxide and corrosion inhibitor 5-amino water were used. Synetic acid extends the diffusion pathway of corrosive media and forms a self-healing barrier.
It significantly improves the corrosion resistance and self-repairing performance of magnesium lithium alloy, forming a uniform and dense film layer, suitable for applications in aerospace, 3C products and automobile industry, with a simple process and environmental protection.
Smart Images

Figure CN118932333A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal surface protection treatment, and specifically relates to a quaternary MgLiAlCe-LDHs@GO-5NH3 film layer on the surface of a magnesium-lithium alloy, and a preparation method and application thereof. Background Art
[0002] As the lightest metal structural material in the world, magnesium-lithium alloy has attracted much attention with the development of industries such as automobiles and 3C products. Its density is generally 1.3-1.65g / cm 3 , it has high specific strength, high specific stiffness, large damping, good seismic performance, good electromagnetic shielding performance, and has broad prospects in the fields of aerospace, weapons industry, nuclear industry, automobile, 3C industry, sports equipment, medical equipment, etc. However, the electrode potential of magnesium-lithium alloy is lower than that of other magnesium alloys, and its corrosion resistance is correspondingly worse. It will also suffer from severe corrosion when placed in a normal temperature atmosphere, which limits its application range. Therefore, improving the corrosion resistance of magnesium-lithium alloy is of great significance for the application and promotion of magnesium-lithium alloy.
[0003] There are two main solutions to the problem of poor corrosion resistance of magnesium-lithium alloys: one is alloying, deformation processing, and heat treatment based on the alloy itself; the other is surface treatment to reduce the impact of the external environment on the metal. However, once the film layer currently used, such as the anodized film, is damaged, the substrate will begin to corrode or even accelerate corrosion, causing the film layer to lose its protective effect.
[0004] LDHs, also known as hydrotalcite-like compounds, is an anionic two-dimensional layered self-healing material, and its structural formula can be expressed as: [M 2+ 1-x M 3+ (OH)2] x+ (A n- ) x / n mH2O, where M 2+ For divalent metal cations, including Zn 2+ , Cu 2+ Mg 2+ etc., M. 3+ is a trivalent metal cation, with Al 3+ Mainly; anion A n- As intercalated anions for structural anion compensation. The current LDHs membrane structure is mostly binary MgAl-LDHs or ZnAl-LDH, which are relatively loose porous structures and cannot effectively isolate the substrate from the external corrosive environment. For example, in the application document with publication number CN117187805A, a method for preparing MgAl-LDHs is proposed, in which a micro-arc oxidation technology is used to construct a micron-sized magnesium oxide layer on the surface of the magnesium alloy as a transition layer; the obtained product contains NO3- The alloy is hydrothermally treated in an alkaline solution at 123-128°C for 14-16 hours, thereby constructing a nano-scale double hydroxy metal hydroxide layer on the surface of the micron-scale magnesium oxide layer, which improves the corrosion resistance of the magnesium alloy to a certain extent.
[0005] There is a common problem with the current LDHs corrosion protection film: LDHs nanosheets generally grow perpendicular to the substrate, and gaps are formed between the sheets, which are porous and can resist corrosive media (Cl - ,O2 and H2O) provide diffusion paths, promote cathode reactions, and affect the corrosion resistance of the film. In view of this problem, introducing doping materials to improve the voids of LDHs nanosheets is an effective solution. Graphene oxide (GO) is a defect-free monolayer material with abundant negative charges on the surface and is impermeable to water and polar solutions. It has good theoretical adaptability to positively charged LDHs. The negatively charged surface of GO shows strong adsorption capacity for metal cations in the solution, and the GO surface has abundant negatively charged functional groups that can provide nucleation sites for the growth of LDHs. LDHs nanosheets can grow on the surface of GO sheets. The disordered distribution of GO sheets can promote the growth of LDHs in multiple directions, so that LDHs are no longer perpendicular to the substrate in large quantities, forming a denser film layer.
[0006] In order to better adapt to the complex and changing environment, the role of corrosion inhibitors has been increasingly valued. Suitable corrosion inhibitors can not only improve the corrosion resistance of the LDHs film, but also form a better self-healing behavior between the LDHs film and the LDHs film. Summary of the invention
[0007] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing quaternary MgLiAlCe-LDHs@GO-5NH3 on the surface of magnesium-lithium alloy;
[0008] The object of the present invention is to provide a quaternary MgLiAlCe-LDHs@GO-5NH3 film on the surface of a magnesium-lithium alloy;
[0009] The purpose of the present invention is to also provide the application of the quaternary MgLiAlCe-LDHs@GO-5NH3 film layer on the surface of the magnesium-lithium alloy in the fields of aerospace, 3C products, and automobile industry.
[0010] The objective of the present invention is achieved through the following technical solutions:
[0011] A method for preparing a MgLiAlCe-LDHs@GO-5NH3 film layer comprises the following steps:
[0012] 1) performing micro-arc oxidation on the surface of the magnesium-lithium alloy to obtain a magnesium-lithium alloy treated with micro-arc oxidation;
[0013] 2) sealing the magnesium-lithium alloy treated by micro-arc oxidation with a cerium ion solution to obtain a magnesium-lithium alloy sealed with a cerium salt;
[0014] 3) immersing the magnesium-lithium alloy sealed with cerium salt obtained in step 2) into a GO growth solution for in-situ growth to obtain a magnesium-lithium alloy with in-situ grown GO, i.e., a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO film layer;
[0015] 4) The magnesium-lithium alloy with in-situ grown GO obtained in step 3) is placed in a corrosion inhibitor solution to load the corrosion inhibitor, thereby obtaining a magnesium-lithium alloy loaded with the corrosion inhibitor, that is, a magnesium-lithium alloy coated with a MgLiAlCe-LDHs@GO-5NH3 film layer.
[0016] In some specific embodiments, the magnesium-lithium alloy before micro-arc oxidation is polished with sandpaper, washed with deionized water and anhydrous ethanol, and then dried after washing.
[0017] In certain specific embodiments, the bath solution of micro-arc oxidation in step 1) includes 0.5-2.5 g / L of sodium hydroxide and 5-10 g / L of sodium aluminate.
[0018] In some specific embodiments, the micro-arc oxidation in step 1) is specifically as follows: stainless steel is used as the cathode, the magnesium-lithium alloy matrix sample is used as the anode, and the distance between the cathode and the anode is ensured to be moderate (5-10 cm), the power supply is a pulsed AC power supply, the constant voltage is 5 min, the voltage is 300 V and the frequency is 500 Hz, the duty cycle is 26%, and it is maintained at 25±5° C. by a water cooling system, and then washed once with deionized water and dried.
[0019] In some specific embodiments, the cerium ion solution in step 2) includes 1-3 g / L cerium nitrate and 0.1-1 g / L hydrogen peroxide; and the process parameters of the sealing treatment in step 2) are: reaction temperature is 45-55°C, and reaction time is 0.75-1.25h.
[0020] In some specific embodiments, the GO growth solution in step 3) includes 0.02-0.03 g / L of graphene oxide and 7-10 g / L of sodium nitrate; and the process parameters of the in-situ growth in step 3) are: the reaction temperature is 80°C-100°C, the pH is 9.5-11.5, and the reaction time is 10-15 h.
[0021] In some specific embodiments, the corrosion inhibitor solution in step 4) is 0.02-0.06M 5-aminosalicylic acid.
[0022] In some specific embodiments, the process parameters of loading the corrosion inhibitor in step 4) are: the reaction temperature is 45° C. to 55° C., the pH is 8.0 to 9.0, and the reaction time is 10 to 15 hours.
[0023] A MgLiAlCe-LDHs@GO-5NH3 film layer obtained by the aforementioned preparation method.
[0024] An application of the aforementioned MgLiAlCe-LDHs@GO-5NH3 film layer or the MgLiAlCe-LDHs@GO-5NH3 film layer prepared by the aforementioned preparation method in the fields of aerospace, 3C products, and automotive industries.
[0025] Compared with the prior art, the present invention has at least the following advantages:
[0026] 1) The preparation method of the MgLiAlCe-LDHs@GO-5NH3 film provided by the present invention uses the micro-arc oxidation film sealed with cerium salt to provide endogenous metal cations, in situ grows the MgLiAlCe-LDHs@GO film in the graphene oxide suspension, and then loads the corrosion inhibitor 5-aminosalicylic acid by anion exchange method to form a dense MgLiAlCe-LDHs@GO-5NH3 film; the introduction of GO promotes the growth of LDHs nanosheets in all directions, the diffusion path of the corrosive medium is extended and tortuous, and the interlayer cations of 5-aminosalicylic acid and LDHs further form a physical barrier on the surface to seal small gaps and defects. At the same time, the preparation method of the present invention uses simple reagents, does not pollute the environment, and the overall process is simple and green.
[0027] 2) The MgLiAlCe-LDHs@GO-5NH3 film provided by the present invention is obtained by in-situ growth and anion exchange, and the MgLiAlCe-LDHs@GO-5NH3 film is introduced by cation Ce and loaded with a specific corrosion inhibitor, so that the corrosion inhibitor 5-aminosalicylic acid reacts with Mg in the surrounding environment. 2+ The cations form chelates such as Mg(5-ASA)2 and precipitate at the damaged part to form a self-repairing film. At the same time, the rare earth cerium ions between the LDHs main layers are also released and react with OH - The cerium hydroxide formed covers the damaged part, further preventing the expansion of corrosion. There is a synergistic effect between the two film layers, which gives the MgLiAlCe-LDHs@GO-5NH3 film layer excellent self-healing properties. The film layer is not only uniform and dense, but also provides excellent corrosion resistance; it is suitable for promotion and application in aerospace, 3C products, automotive industry and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0029] Figure 1 is a scanning electron microscope photograph of the surface of the magnesium-lithium alloy after micro-arc oxidation in Example 1;
[0030] Figure 2 is a scanning electron microscope photograph of the magnesium-lithium alloy MgLiAl-LDHs@GO film layer in Example 1;
[0031] Figure 3 is a scanning electron microscope photograph of the magnesium-lithium alloy MgLiAlCe-LDHs@GO film layer obtained in Example 1;
[0032] Figure 4 is the XRD spectrum of the magnesium-lithium alloy MgLiAlCe-LDHs@GO film layer obtained in Example 1 under the pH value condition;
[0033] Figure 5 This is the FT-IR spectrum of the magnesium-lithium alloy MgLiAlCe-LDHs@GO film obtained in Example 1 under the pH value condition;
[0034] Figure 6 This is a scanning electron microscope photograph of the MgLiAlCe-LDHs@GO film layer loaded with 0.02M 5-aminosalicylic acid on the magnesium-lithium alloy obtained in Example 2;
[0035] Figure 7 The XRD spectra of the MgLiAlCe-LDHs@GO film layer loaded with 0.02M 5-aminosalicylic acid and the MgLiAlCe-LDHs@GO film layer of the magnesium-lithium alloy obtained in Example 2 under the pH value condition;
[0036] Figure 8 This is a scanning electron microscope photograph of the MgLiAlCe-LDHs@GO film layer loaded with 0.06M 5-aminosalicylic acid on the magnesium-lithium alloy obtained in Example 3;
[0037] Fig. 9 The XRD spectra of the MgLiAlCe-LDHs@GO film layer loaded with 0.06M 5-aminosalicylic acid and the MgLiAlCe-LDHs@GO film layer of the magnesium-lithium alloy obtained in Example 3 under the pH condition;
[0038] Fig.10 This is a scanning electron microscope photograph of the MgLiAlCe-LDHs@GO film layer loaded with 0.04M 5-aminosalicylic acid on the magnesium-lithium alloy obtained in Example 4;
[0039] Fig.11 The XRD spectra of the MgLiAlCe-LDHs@GO film layer loaded with 0.04M 5-aminosalicylic acid and the MgLiAlCe-LDHs@GO film layer of the magnesium-lithium alloy obtained in Example 4 under the pH condition;
[0040] Fig.12 The Mg-8Li alloy covered with a micro-arc oxidation film (MAO curve), the Mg-8Li alloy covered with a MgLiAl-LDHs@GO film layer, the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO film layer, and the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO film layer measured by an electrochemical workstation in Examples 1-4
[0041] Mg-8Li alloy of MgLiAlCe-LDHs@GO-5NH3-2 film, covered with
[0042] Tafel polarization curves of MgLiAlCe-LDHs@GO-5NH3-6 and Mg-8Li alloy coated with MgLiAlCe-LDHs@GO-5NH3-4 film at the same coordinates;
[0043] Fig.13 The surface morphology and EDS spectra of the scratches of Mg-8Li alloy covered with micro-arc oxidation film, Mg-8Li alloy covered with MgLiAlCe-LDHs@GO film, and Mg-8Li alloy covered with MgLiAlCe-LDHs@GO-5NH3-4 film before and after immersion in 3.5wt.% NaCl solution for 24 hours. DETAILED DESCRIPTION
[0044] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0045] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0046] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0047] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0048] The present invention provides a general and / or specific description of the materials and test methods used in the experiment. The test methods or test methods involved are all conventional methods unless otherwise specified; the reagents or instruments used are all conventional products available on the market, prepared or used in a conventional manner, unless the manufacturer is specified.
[0049] In the following embodiments, Mg-8Li is used as an example for explaining the magnesium-lithium alloy. The magnesium-lithium alloy before micro-arc oxidation is polished with sandpaper to 2000#, washed with deionized water and anhydrous ethanol, and then dried for use.
[0050] Example 1
[0051] This embodiment provides a method for preparing a MgLiAl-LDHs@GO film layer on a magnesium-lithium alloy surface, comprising the following steps:
[0052] 1) Micro-arc oxidation
[0053] 11) Prepare micro-arc oxidation tank liquid:
[0054] Prepare a micro-arc oxidation tank solution containing 1.5 g / L sodium hydroxide and 7 g / L sodium aluminate;
[0055] 12) Micro-arc oxidation:
[0056] Stainless steel was used as cathode, magnesium-lithium alloy (Mg-8Li alloy) matrix sample was used as anode, and the distance between cathode and anode was ensured to be at a moderate distance of 5-10 cm. The power supply was a pulsed AC power supply, constant voltage for 5 min, voltage was 300 V, frequency was 500 Hz, duty cycle was 26%, and maintained at 25±5°C by a water cooling system. The last step was to wash once with deionized water and dry in air to obtain magnesium-lithium alloy with micro-arc oxidation film (MAO curve).
[0057] 2) Cerium salt sealing
[0058] 21) Preparation of cerium ion solution
[0059] Prepare a cerium ion solution containing 2 g / L cerium nitrate and 0.5 g / L hydrogen peroxide;
[0060] 22) Closed processing
[0061] The magnesium-lithium alloy subjected to micro-arc oxidation was placed in a cerium ion solution for reaction at a temperature of 50° C. for a reaction time of 1 h to obtain a magnesium-lithium alloy sealed with a cerium salt.
[0062] 3) In situ growth of MgLiAlCe-LDHs@GO film
[0063] 31) Preparation of GO growth solution
[0064] Prepare a GO growth solution containing 0.02 g / L graphene oxide and 8.5 g / L sodium nitrate;
[0065] 32) In situ growth
[0066] The cerium salt-sealed magnesium-lithium alloy obtained in step 2) is immersed in a GO growth solution for in-situ growth, wherein the reaction temperature is 90° C., the pH value is 10.5, and the reaction time is 12 h, to obtain a magnesium-lithium alloy with in-situ growth of GO (MgLiAlCe-LDHs@GO film layer);
[0067] 4) Clean and dry
[0068] The magnesium-lithium alloy with in-situ GO growth in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes using an ultrasonic cleaner, and then cleaned with deionized water and dried to obtain a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO film layer.
[0069] At the same time, this application also introduces a comparative example:
[0070] The preparation of the membrane layer (MgLiAl-LDHs@GO membrane layer) without Ce sealing treatment in the technical solution of this comparative example specifically includes the following steps:
[0071] 1) Micro-arc oxidation
[0072] 11) Prepare micro-arc oxidation tank liquid:
[0073] Prepare a micro-arc oxidation tank solution containing 1.5 g / L sodium hydroxide and 7 g / L sodium aluminate;
[0074] 12) Micro-arc oxidation:
[0075] Stainless steel was used as cathode, Mg-8Li alloy matrix sample was used as anode, and the distance between cathode and cathode was ensured to be moderate. The power supply was pulse AC power supply, constant voltage for 5min, voltage was 300v, frequency was 500Hz, duty cycle was 26%, and it was kept at 25±5℃ by water cooling system. The last step was to wash once with deionized water and dry in air to obtain magnesium-lithium alloy treated by micro-arc oxidation.
[0076] 2) In situ growth of MgLiAl-LDHs@GO film
[0077] 31) Preparation of GO growth solution
[0078] Prepare a GO growth solution containing 0.02 g / L graphene oxide and 8.5 g / L sodium nitrate;
[0079] 32) In situ growth
[0080] The magnesium-lithium alloy treated with micro-arc oxidation obtained in step 2) is immersed in a GO growth solution for in-situ growth, wherein the reaction temperature is 90° C., the pH value is 10.5, and the reaction time is 12 h, to obtain a magnesium-lithium alloy with in-situ growth of GO (MgLiAl-LDHs@GO film layer);
[0081] 4) Clean and dry
[0082] The magnesium-lithium alloy with in-situ GO growth in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes using an ultrasonic cleaner, and then cleaned with deionized water and dried to obtain a magnesium-lithium alloy covered with a MgLiAl-LDHs@GO film layer.
[0083] The present application uses a scanning electron microscope to analyze the microstructure of the micro-arc oxidation film layer (MAO curve) on the surface of the magnesium-lithium alloy in Example 1, the MgLiAl-LDHs@GO film layer (comparative example), and the MgLiAlCe-LDHs@GO film layer. The results are as follows: Figure 1 , Figure 2 and Figure 3 As shown in the figure, it can be seen that the surface of the micro-arc oxidation film has a characteristic volcanic pore morphology, and the porosity is high, which provides a path for the diffusion of the corrosive medium; with the introduction of GO, its negatively charged surface will adsorb the cations released by the dissolution of the micro-arc oxidation film, providing more nucleation sites for the growth of LDHs nanosheets, and finally the obtained film layer is denser and the porosity is reduced; due to Ce 3+ Radius Ratio Al 3+ Large radius, Al 3+ Be Ce 3+ Isomorphous substitution will cause LDHs lattice distortion. The nanosheets of the MgLiAlCe-LDHs@GO film are larger and more oblate, and are relatively thicker and more compact in structure with almost no obvious pores, making the medium conduction path more tortuous and greatly extending the erosion path of corrosive substances.
[0084] The present application also performed XRD scanning analysis on the MgLiAlCe-LDHs@GO film layer in Example 1. The results are as follows: Figure 4 As shown in the figure, the diffraction peaks of the characteristic crystal planes (003) and (006) of the MgLiAlCe-LDHs@GO film are located near 11° and 23°, respectively. The present application also conducted FT-IR scanning tests on the MgLiAlCe-LDHs@GO film, and the results are as follows: Figure 5 As shown in the figure, it can be seen that the MgLiAlCe-LDHs@GO film has a tensile vibration generated by C=C / CC. Figure 4 and Figure 5It can be seen that this embodiment successfully formed a MgLiAlCe-LDHs@GO film layer on the surface of the magnesium-lithium alloy.
[0085] Example 2
[0086] This embodiment provides a method for preparing a MgLiAlCe-LDHs@GO-5NH3-2 film layer on a magnesium-lithium alloy surface, wherein steps 1) to 3) are the same as those in embodiment 1, except that a step of loading a corrosion inhibitor is added, specifically:
[0087] 4) placing the magnesium-lithium alloy with in-situ grown GO in step 3) in a 0.02M 5-aminosalicylic acid solution for loading reaction, the reaction temperature is 50° C., pH 8.5, and the reaction time is 12 h to obtain a magnesium-lithium alloy loaded with corrosion inhibitor (MgLiAlCe-LDHs@GO-5NH3-2 film layer);
[0088] 5) Clean and dry
[0089] The magnesium-lithium alloy loaded with the corrosion inhibitor in step 4) is first cleaned with flowing deionized water to remove the corrosion inhibitor solution attached to the surface, and then placed in an ultrasonic cleaning machine for ultrasonic cleaning in anhydrous ethanol for 5 minutes, and then cleaned with deionized water and dried to obtain a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO-5NH3-2 film layer.
[0090] The present application conducts a performance test on the MgLiAlCe-LDHs@GO-5NH3-2 film layer prepared in this embodiment, specifically:
[0091] 1. Morphology and organization test
[0092] The present application uses metallographic microscope and scanning electron microscope to analyze the microstructure of the MgLiAlCe-LDHs@GO-5NH3-2 film in Example 2. The results are as follows: Figure 6 As shown in the figure, it can be seen that there is a slight connection between the nanosheets on the MgLiAlCe-LDHs@GO-5NH3-2 film layer, and a small amount of particles are adsorbed on the LDHs, which may be a small amount of chelate formed by metal cations and corrosion inhibitors. ;
[0093] The present application also performs XRD scanning analysis on the MgLiAlCe-LDHs@GO film layer and the MgLiAlCe-LDHs@GO-5NH3-2 film layer in Example 2. The results are as follows: Figure 7 As shown in the figure, it can be seen that the (003) and (006) characteristic crystal plane diffraction peaks of the MgLiAlCe-LDHs@GO-5NH3-2 film layer are shifted to the left compared with the MgLiAlCe-LDHs@GO film layer, indicating that the corrosion inhibitor is successfully inserted into the LDHs layer.
[0094] Example 3
[0095] This embodiment provides a method for preparing a MgLiAlCe-LDHs@GO-5NH35NH3-6 film layer on a magnesium-lithium alloy surface, which is basically the same as that of Example 2, except that the molar concentration of the corrosion inhibitor-aminosalicylic acid solution is 0.06M, specifically:
[0096] 4) placing the magnesium-lithium alloy with in-situ grown GO in step 3) in a 0.06M 5-aminosalicylic acid solution for loading reaction, the reaction temperature is 50° C., pH 8.5, and the reaction time is 12 h to obtain a magnesium-lithium alloy loaded with corrosion inhibitor (MgLiAlCe-LDHs@GO-5NH3-6 film layer);
[0097] 5) Clean and dry
[0098] The magnesium-lithium alloy loaded with the corrosion inhibitor in step 4) is first cleaned with flowing deionized water to remove the corrosion inhibitor solution attached to the surface, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO-5NH3-6 film layer.
[0099] 1. Morphology and organization test
[0100] The present application uses metallographic microscope and scanning electron microscope to analyze the microstructure of the MgLiAlCe-LDHs@GO-5NH3-6 film in Example 3. The results are as follows: Figure 8 As shown in the figure, it can be seen that the MgLiAlCe-LDHs@GO-5NH3-6 film has a higher density than the MgLiAlCe-LDHs@GO film, and the integrity of the surface nanosheets is also higher;
[0101] The present application also performs XRD scanning analysis on the MgLiAlCe-LDHs@GO film layer and the MgLiAlCe-LDHs@GO-5NH35NH3-6 film layer in Example 3. The results are as follows: Fig. 9 As shown in the figure, it can be seen that the (003) and (006) characteristic crystal plane diffraction peaks of the MgLiAlCe-LDHs@GO-5NH35NH3-6 film layer are shifted to the left compared with the MgLiAlCe-LDHs@GO film layer, indicating that the corrosion inhibitor is successfully inserted into the LDHs layer.
[0102] Example 4
[0103] This embodiment provides a method for preparing a MgLiAlCe-LDHs@GO-5NH35NH3-4 film layer on a magnesium-lithium alloy surface, which is basically the same as that of Example 2, except that the molar concentration of the corrosion inhibitor-aminosalicylic acid solution is 0.04M, specifically:
[0104] 4) placing the magnesium-lithium alloy with in-situ grown GO in step 3) in a 0.04M 5-aminosalicylic acid solution for loading reaction, the reaction temperature is 50° C., pH 8.5, and the reaction time is 12 h to obtain a magnesium-lithium alloy loaded with corrosion inhibitor (MgLiAlCe-LDHs@GO-5NH3-4 film layer);
[0105] 5) Clean and dry
[0106] The magnesium-lithium alloy loaded with the corrosion inhibitor in step 4) is first cleaned with flowing deionized water to remove the corrosion inhibitor solution attached to the surface, and then ultrasonically cleaned in anhydrous ethanol for 5 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO-5NH3-4 film layer.
[0107] The present application uses metallographic microscope and scanning electron microscope to analyze the microstructure of the MgLiAlCe-LDHs@GO-5NH35NH3-4 film in Example 4. The results are as follows: Fig.10 As shown in the figure, it can be seen that there is an obvious connection phenomenon on the surface of the MgLiAlCe-LDHs@GO-5NH3-4 film, forming a physical barrier, which further fills the gaps and hinders the erosion of corrosive media.
[0108] The present application also performs XRD scanning analysis on the MgLiAlCe-LDHs@GO film layer and the MgLiAlCe-LDHs@GO-5NH35NH3-4 film layer in Example 4. The results are as follows: Fig.11 As shown in the figure, it can be seen that the (003) and (006) characteristic crystal plane diffraction peaks of the MgLiAlCe-LDHs@GO-5NH35NH3-4 film layer are shifted to the left compared with the MgLiAlCe-LDHs@GO film layer, indicating that the corrosion inhibitor is successfully inserted into the LDHs layer.
[0109] This application takes Examples 1-4 as an example to test the corrosion resistance of the prepared film layer, and the results are:
[0110] 1) Electrochemical corrosion test
[0111] The corrosion resistance test of the film layer is represented by an electrochemical polarization curve (the equipment is P4000a). The present application measured by an electrochemical workstation the Tafel polarization curves of the Mg-8Li alloy covered with a micro-arc oxidation film (MAO curve), the Mg-8Li alloy covered with a MgLiAl-LDHs@GO closed film layer (Comparative Example 1), the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO film layer, the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO-5NH3-2 film layer, the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO-5NH3-6 film layer, and the Mg-8Li alloy covered with a MgLiAlCe-LDHs@GO-5NH3-4 film layer under the same coordinates. The results are as follows Fig.12 As shown in the figure, we can see that:
[0112] The corrosion current density of the Mg-8Li alloy covered only with micro-arc oxidation film is 5.09×10 -6 Acm -2 The corrosion current density of the MgLiAl-LDHs@GO closed film layer without Ce ions (comparative example) is 5.72×10 -7 Acm -2 The corrosion current density of the Mg-8Li alloy in the MgLiAlCe-LDHs@GO closed film layer after treatment under the conditions of Example 1 is 3.27×10 - 8 Acm -2 The corrosion current density of the treated samples was reduced by two orders of magnitude compared with that of the samples oxidized by micro-arc oxidation. Compared with the Mg-8Li alloy with micro-arc oxidation film, it can be seen that graphene oxide effectively changes the vertical growth state of most LDHs nanosheets and effectively closes the gaps. The MgLiAlCe-LDHs@GO-film layer on the surface of the magnesium-lithium alloy of the present invention can effectively protect the substrate.
[0113] The corrosion current density of the Mg-8Li alloy with the MgLiAlCe-LDHs@GO-5NH3-2 closed film after treatment under the conditions of Example 2 is 1.66×10 -8 Acm -2 The corrosion current density of the MgLiAlCe-LDHs@GO-5NH3-6 closed film after treatment under the conditions of Example 3 is 8.54×10 -9 Acm -2 The corrosion current density of the MgLiAlCe-LDHs@GO-5NH3-4 closed film after treatment under the conditions of Example 4 is 5.61×10 -9 Acm -2Among them, the corrosion current density of the sample treated under the conditions of Example 4 is most significantly reduced compared with the MgLiAlCe-LDHs@GO closed film layer.
[0114] In summary, the corrosion current density of the Mg-8Li alloy after the MgLiAlCe-LDHs@GO-5NH3 closed film layer loaded with corrosion inhibitor is further reduced. The above results can be explained as the loading of 0.02M, 0.04M, and 0.06M 5-aminosalicylic acid forms a physical barrier on the surface of the film layer, filling the gaps, closing or blocking defects, and effectively enhancing the corrosion resistance of the film layer. The MgLiAlCe-LDHs@GO-5NH3 film layer on the surface of the magnesium-lithium alloy of the present invention can effectively protect the substrate.
[0115] 2) Chemical corrosion test
[0116] The present invention tests the surface morphology and EDS spectrum of the scratched Mg-8Li alloy coated with micro-arc oxidation film, the Mg-8Li alloy coated with MgLiAlCe-LDHs@GO film, and the Mg-8Li alloy coated with MgLiAlCe-LDHs@GO-5NH3-4 film before and after immersion in 3.5wt.% NaCl solution for 24h. The results are as follows: Fig.13 As shown in the figure, the scratched area of the MgLiAl-LDHs@GO film has a slight tendency of corrosion diffusion. According to the EDS spectrum, the corrosion products may be composed of magnesium-containing compounds such as Mg(OH)2; the scratched area of the MgLiAlCe-LDH@GO film has a relatively denser precipitate to fill it. According to the metallographic diagram, the precipitate may be a mixture of cerium hydroxide and magnesium-containing compounds; the scratched area of the MgLiAlCe-LDHs@GO-5NH3-4 film is almost completely covered by corrosion products, and the distribution of corrosion products is uniform and dense. Combined with the EDS spectrum, the N content is 3.5at.%, which is significantly higher than that of other film layers. This is because 5-aminosalicylic acid forms chelates such as Mg(5-ASA)2 with cations in the surrounding environment and precipitates at the damaged area to form a self-repairing film layer. In addition, the rare earth cerium ions between the LDHs main layer plates are also released and react with OH - The cerium hydroxide formed covers the damaged area, further preventing the expansion of corrosion. There is a synergistic effect between the two film layers, which gives the MgLiAlCe-LDHs@GO-5NH3-4 film layer excellent self-healing properties.
[0117] In summary: The inventors have verified through a large number of experiments and found that the micro-arc oxidation film sealed with Mg-8Li alloy cerium salt is used as a cation source, the MgLiAlCe-LDHs@GO film layer is in situ grown in a graphene oxide suspension, and the corrosion inhibitor 5-aminosalicylic acid is loaded to obtain a MgLiAlCe-LDHs@GO-5NH3 film layer with a more tortuous diffusion path of the corrosive medium. The introduction of graphene oxide promotes the growth of LDHs nanosheets in all directions, and the diffusion path of the corrosive medium is extended and tortuous. The interlayer cations of 5-aminosalicylic acid and LDHs further form a physical barrier on the surface, closing small gaps and defects. The rare earth cerium ions with corrosion inhibition effect and the corrosion inhibitor anions can work synergistically, thereby effectively blocking and preventing external corrosive ions (such as Cl - The process is easy to operate, simple and environmentally friendly. It is a green and safe process for preparing a high corrosion-resistant film on the surface of magnesium-lithium alloy.
[0118] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a MgLiAlCe-LDHs@GO-5NH3 film, characterized in that: The steps include: 1) performing micro-arc oxidation on the surface of the magnesium-lithium alloy to obtain a magnesium-lithium alloy treated with micro-arc oxidation; 2) sealing the magnesium-lithium alloy treated by micro-arc oxidation with a cerium ion solution to obtain a magnesium-lithium alloy sealed with a cerium salt; 3) immersing the magnesium-lithium alloy sealed with cerium salt obtained in step 2) into a GO growth solution for in-situ growth to obtain a magnesium-lithium alloy with in-situ grown GO, i.e., a magnesium-lithium alloy covered with a MgLiAlCe-LDHs@GO film layer; 4) The magnesium-lithium alloy with in-situ grown GO obtained in step 3) is placed in a corrosion inhibitor solution to load the corrosion inhibitor, thereby obtaining a magnesium-lithium alloy loaded with the corrosion inhibitor, that is, a magnesium-lithium alloy coated with a MgLiAlCe-LDHs@GO-5NH3 film layer.
2. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 1, characterized in that: The method also includes grinding the magnesium-lithium alloy before micro-arc oxidation with sandpaper, washing with deionized water, washing with anhydrous ethanol, and then drying after washing.
3. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 1, characterized in that: In step 1), the bath solution of micro-arc oxidation includes 0.5-2.5 g / L of sodium hydroxide and 5-10 g / L of sodium aluminate.
4. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 1, characterized in that: In step 1), micro-arc oxidation is specifically as follows: stainless steel is used as the cathode, the magnesium-lithium alloy matrix sample is used as the anode, and the distance between the cathode and the anode is ensured to be 5-10 cm. The power supply is a pulsed AC power supply, constant voltage for 5 minutes, the voltage is 300 V and the frequency is 500 Hz, the duty cycle is 26%, and it is maintained at 25±5°C through a water cooling system, and then washed once with deionized water and dried.
5. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 4, characterized in that: The cerium ion solution in step 2) includes 1-3 g / L cerium nitrate and 0.1-1 g / L hydrogen peroxide; and the process parameters of the sealing treatment in step 2) are: reaction temperature is 45-55° C., and reaction time is 0.75-1.25 h.
6. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 1, characterized in that: The GO growth solution in step 3) includes 0.02-0.03 g / L of graphene oxide and 7-10 g / L of sodium nitrate; and the process parameters of the in-situ growth in step 3) are: the reaction temperature is 80° C. to 100° C., the pH is 9.5-11.5, and the reaction time is 10-15 h.
7. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 1, characterized in that: The corrosion inhibitor solution in step 4) is 0.02-0.06M 5-aminosalicylic acid.
8. The method for preparing the MgLiAlCe-LDHs@GO-5NH3 film according to claim 4, characterized in that: The process parameters of loading the corrosion inhibitor in step 4) are: reaction temperature of 45°C to 55°C, pH 8.0 to 9.0, and reaction time of 10 to 15 hours.
9. A MgLiAlCe-LDHs@GO-5NH3 film obtained by the preparation method according to any one of claims 1-8.
10. Application of the MgLiAlCe-LDHs@GO-5NH3 film according to claim 9 in the fields of aerospace, 3C products, and automobile industry.