Molten salt electrochemical preparation method of iron-titanium alloy powder

Through the molten salt electrochemical method, the problems of three waste emissions and many impurities in the preparation of iron-titanium alloys are solved, and high-purity and low-carbon iron-titanium alloys are prepared are achieved, meeting the requirements of green circular economy.

CN118932431APending Publication Date: 2024-11-12NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110704.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing iron-titanium alloy preparation technology has problems such as three waste emissions, complex links, many impurities, and low purity, making it difficult to achieve a green, low-carbon and short-process preparation method.

Method used

Using molten salt electrochemical method, iron-containing raw material powder is mixed with alkali metal or alkaline earth metal inorganic salts and active components, dried and constant temperature electrolyzed to form an anhydrous furnace material, and then heated to liquid under an inert atmosphere, setting the voltage Electrolysis was performed to form a ferrotitanium alloy, which was then washed with deionized water and anhydrous ethanol and dried in vacuo to obtain a ferrotitanium alloy powder.

Benefits of technology

It realizes effective separation of raw materials, and prepares high-purity iron-titanium alloys, avoids pollution and carbon emissions, meets the needs of low-carbon green circular economy, has short processes, low equipment requirements, and the product has no impurity residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932431A_ABST
    Figure CN118932431A_ABST
Patent Text Reader

Abstract

The invention discloses a molten salt electrochemical preparation method of iron-titanium alloy powder. The method comprises the following steps: 1, drying a mixture containing iron and titanium raw materials, alkali metal or / and alkaline earth metal inorganic salt and active components to obtain furnace charge; 2, under a two-electrode system, heating and melting the furnace charge into a liquid molten salt system, and then continuously electrolyzing; and 3, stripping the cathode product, alternately soaking the cathode product in deionized water and absolute ethyl alcohol, performing ultrasonic cleaning, and drying to obtain a product, namely the iron-titanium alloy. According to the method, the raw material powder containing iron and titanium, the alkali metal or / and alkaline earth metal inorganic salt and the active component are mixed and melted and then are electrolyzed at constant voltage, and iron and titanium electroactive ions in the mixed molten salt are continuously discharged on a cathode and are co-electrodeposited on the cathode, so that an iron-titanium alloy product is obtained, and green short-process co-electroreduction of iron and titanium is realized; and in the electrolysis process, green energy can be used for supplying energy, the process is simple and controllable, operation is safe, environment friendliness is achieved, and the technological thought of molten salt electrochemistry in the aspect of alloy preparation is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material chemistry, in particular to the field of material preparation, and specifically to a molten salt electrochemical preparation method of an iron-titanium alloy. Background Art

[0002] With the continuous development of society, the use of green and sustainable energy has attracted much attention from all parties. As a recognized clean energy, the green preparation, storage and transportation of hydrogen energy are of great significance to the practical use of hydrogen energy. Hydrogen storage alloys are called hydrogen sponges because the density of hydrogen stored is greater than that of liquid hydrogen. Among them, iron-titanium alloys are widely studied as titanium-based hydrogen storage alloys because of their large hydrogen absorption capacity and rapid hydrogen absorption and release.

[0003] At present, the main preparation technologies of ferro-titanium alloy include aluminothermic reduction, carbon thermal reduction, metal remelting, etc., among which aluminothermic reduction accounts for a large proportion. The pyrometallurgical process inevitably has process problems such as three wastes discharge and complex links. In addition, there are reports (Nonferrous Metals, 2019, 6(5):50-55) pointing out that the ferro-titanium alloy obtained by this method still contains a large amount of impurities. Therefore, in response to my country's green and sustainable energy utilization strategy, how to achieve the preparation of ferro-titanium alloy with a short process and green near-zero emission technology has become a technical difficulty to be overcome.

[0004] Molten salt electrochemical technology uses high-temperature molten salt as an ion conductor. Since high-temperature molten salt has a wide electrochemical window and fast reaction kinetics at high temperatures, it is an ideal electrolyte system for electrochemical metallurgy, and the electrolytic aluminum industry is a successful example. In recent years, the most famous is the FFC process, which proposes that in a CaCl2 molten salt system, TiO2 is directly used as a solid cathode and graphite is used as an electrolytic anode for cathode electro-deoxidation, thereby obtaining a single sponge titanium at the cathode (Metallurgical and Materials Transcation B, 2001, 32 (6): 1041-1052). In addition, Du Jihong et al. (patent application number 200910021842.4) disclosed a method for preparing ferro-titanium alloy from ilmenite based on the FFC process. The essence of the method is to first calcine ilmenite powder at high temperature to prepare a pressed block cathode, and then perform cathode electro-deoxidation in molten salt to obtain the primary product and then perform vacuum smelting to prepare ferro-titanium alloy. Similarly, Zhou Zhongren (Nonferrous Metals Engineering, 2017, 7(01): 1-5) proposed to directly use FeTiO3 powder as a pressed block cathode and directly electrolyze in molten salt to perform cathode electro-deoxidation to obtain ferro-titanium alloy. The above are essentially the development and extension of the FFC process technology. However, there are reports that this process idea generally has problems such as limited processing capacity, poor deoxidation kinetics at the solid-liquid interface, much residual raw materials, and limited purity of ferro-titanium alloy. Different from the FFC process in essence, this technology discloses a molten salt electrochemical preparation method of ferro-titanium alloy. The detailed technical advantages are introduced as follows. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a molten salt electrochemical preparation method of ferro-titanium alloy in view of the deficiencies of the above-mentioned prior art. The method fully realizes the effective separation of iron and titanium elements in the raw materials, can directly prepare ferro-titanium alloy, uses sustainable energy throughout the process, and has no pollution and carbon-containing gas emissions. It solves the problems of high acid consumption, high pollution, difficult by-product treatment, and high equipment requirements in the traditional ferro-titanium alloy preparation process, avoids the shortcomings of FFC technology, and also meets the current development needs of low-carbon green circular economy.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a molten salt electrochemical preparation method of iron-titanium alloy powder, characterized in that the method comprises the following steps:

[0007] Step 1: Place the mixture of iron- and titanium-containing raw material powders, alkali metal and / or alkaline earth metal inorganic salts, and active components in a crucible, and then place it in a constant temperature drying oven for drying to obtain anhydrous furnace charge; the drying temperature is not less than 100° C., and the drying time is not less than 10 hours;

[0008] Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tubular resistance furnace, heat it to the electrolysis temperature under an inert atmosphere and keep it warm. After the charge is melted into a liquid melt, slowly move the cathode electrode and the anode electrode from the top of the vertical tubular resistance furnace to below the liquid surface of the molten salt system and fix them. Set a voltage of 1.0V to 5.0V between the cathode electrode and the anode electrode. After continuous electrolysis for a period of time, lift each electrode from the liquid surface of the molten salt system and slowly cool it to room temperature as the furnace temperature decreases. The electrolysis temperature is 400°C to 1000°C, and the insulation time before the cathode electrode and the anode electrode are moved to below the liquid surface of the molten salt system is 10min to 30min.

[0009] Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2 is completed, and then soak and wash it alternately with deionized water and anhydrous ethanol for at least 3 times, each washing is performed using an ultrasonic machine for not less than 30 minutes, and the filtrate is obtained by filtration and separation, and the filtrate is transferred to a vacuum drying oven for drying to obtain an iron-titanium alloy powder.

[0010] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that the iron- and titanium-containing raw material powder in step one is a composite of one or more of FeO, Fe2O3, TiO2, FeTiO3, Na2Ti3O7, MgTiO3, Na2FeO4, and CaTiO3, and all contain iron and titanium elements, and the particle size of the iron- and titanium-containing raw material powder is not greater than 0.074 μm.

[0011] In the above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder, when the iron-containing and titanium-containing raw material powders are two different substances, the mass ratio of the iron-containing raw material powder to the titanium-containing raw material powder is 0.5-2.0:1.

[0012] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that, calculated by mass fraction, the total amount of iron- and titanium-containing raw material powders added to the mixture in step one does not exceed 10%.

[0013] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that the alkali metal and / or alkaline earth metal inorganic salt in step one is one or more of LiCl, NaCl, KCl, CsCl, CaCl2, MgCl2, BaCl2, Na2CO3, Li2CO3, K2CO3, Cs2CO3 and BaCO3.

[0014] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that the active component in step one is one of Li2O, CaO and BaO, and the amount of the active component added to the mixture does not exceed 10% of the mass of the alkali metal and / or alkaline earth metal inorganic salt.

[0015] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that the anode electrode in step 2 is a NiFe2O4-based, TiB2-based, SnO2 or RuO2*TiO2 inert electrode, and the cathode electrode is made of nickel, molybdenum or stainless steel.

[0016] The RuO2*TiO2 inert electrode in the present invention means that the RuO2*TiO2 inert electrode is composed of two components, RuO2 and TiO2.

[0017] The above-mentioned molten salt electrochemical preparation method of iron-titanium alloy powder is characterized in that the electrolysis temperature in step 2 is 450°C to 900°C, the voltage between the cathode and anode electrodes is 2.0V to 3.5V, and the electrolysis time is not less than 5h.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] 1. The present invention directly mixes iron- and titanium-containing raw material powders with alkali metal or / and alkaline earth metal inorganic salts and active components, and then heats and performs constant-pressure electrolysis, so that the electrically active iron and titanium ions in the liquid molten salt are discharged and reduced at the cathode to form an iron-titanium alloy, wherein there is no raw material residue in the product, no harmful three wastes are discharged, and there is no pollution to the environment. The whole process avoids the use of strong acids and strong alkalis, is green and environmentally friendly, and meets the current development needs of a low-carbon, green, circular economy.

[0020] 2. The present invention uses non-carbon inert materials as anode electrode materials for electrolysis, further avoiding the generation of greenhouse gas CO2 and the introduction of impurities, which is beneficial to ensure that no impurities remain in the ferro-titanium alloy product.

[0021] 3. The present invention realizes directional control of the composition and micromorphology of the ferro-titanium alloy product by adjusting the process parameters of constant-voltage electrolysis such as voltage, temperature and electrolysis time. It is flexible, convenient and easy to implement.

[0022] 4. The process of the present invention is short. When industrialized, the continuous output of iron-titanium alloy products can be achieved by continuously adding iron- and titanium-containing raw material powders and rotating cathode electrodes, and it has good development prospects in continuous industrial applications.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a physical picture of the cathode electrode after electrolysis is completed in Example 1 of the present invention.

[0025] Figure 2 This is the XRD diagram of the iron-titanium alloy powder obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] Example 1

[0027] This embodiment includes the following steps:

[0028] Step 1: 3.0 g of FeTiO3 powder with a particle size not greater than 0.074 μm, 200 g of CaCl2-NaCl eutectic salt (wherein the molar ratio of CaCl2 to NaCl is 0.53:0.47), and 2.0 g of MgO active component are mixed uniformly and placed in a crucible, and then placed in a drying oven at a temperature of 120° C. for 12 hours to obtain anhydrous furnace charge;

[0029] Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tube resistance furnace, heat to 800°C in an inert atmosphere and keep warm for 10 minutes. After the charge is melted into a liquid melt, slowly move the cathode electrode and the anode electrode from the top of the vertical tube resistance furnace to below the liquid surface of the molten salt system and fix them. Set the voltage between the stainless steel cathode electrode and the tin oxide anode electrode to 2.8V. After continuous electrolysis for 8 hours, lift each electrode from the liquid surface of the molten salt system and slowly drop to room temperature as the furnace temperature drops.

[0030] Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2 is completed, and then soak and wash it alternately with deionized water and anhydrous ethanol for 3 times, each washing is performed using an ultrasonic machine for 30 minutes, and the filtrate is obtained by filtration and separation, and then the filtrate is transferred to a vacuum drying oven for drying for 12 hours to obtain an iron-titanium alloy powder.

[0031] The anode electrode in this embodiment may also be a NiFe2O4-based, TiB2-based, RuO2*TiO2 inert electrode other than the SnO2 anode electrode, and the cathode electrode material may also be nickel or molybdenum.

[0032] Figure 1 This is a physical picture of the cathode electrode after electrolysis is completed in this embodiment. Figure 1 It can be seen that this embodiment uses a molten salt electrochemical method to achieve the deposition of the product iron-titanium alloy on the cathode electrode.

[0033] Figure 2 The XRD diagram of the iron-titanium alloy powder obtained in this embodiment is shown in the figure from top to bottom, which are the XRD diagram of the iron-titanium alloy powder obtained in this embodiment, the PDF card of the standard phase Fe2Ti, the PDF card of the standard phase TiFe, the PDF card of the standard phase Fe, and the PDF card of the standard phase Figure 2 It can be seen that composite phases such as Fe, Fe2Ti, and FeTi exist in the cathode product, indicating that the present invention successfully obtains an iron-titanium alloy phase by using a molten salt electrochemical method.

[0034] Example 2

[0035] This embodiment includes the following steps:

[0036] Step 1: Place a mixture of 1.0 g of Na2FeO4 and 2.0 g of CaTiO3 powder with a particle size of no more than 0.074 μm, 200 g of CaCl2-NaCl eutectic salt (wherein the molar ratio of CaCl2 to NaCl is 0.53:0.47), and 15.0 g of CaO active component in a crucible, and then place the mixture in a drying oven at a temperature of 120° C. for 15 hours to obtain anhydrous furnace charge;

[0037] Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tube resistance furnace, heat to 900°C in an inert atmosphere and keep warm for 30 minutes. After the charge is melted into a liquid melt, slowly move the cathode electrode and the anode electrode from the top of the vertical tube resistance furnace to below the liquid surface of the molten salt system and fix them. Set the voltage between the nickel cathode electrode and the NiFe2O4-based anode electrode to 2.0V. After continuous electrolysis for 5 hours, lift each electrode from the liquid surface of the molten salt system and slowly drop to room temperature as the furnace temperature drops.

[0038] Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2, and then soak and wash it alternately with deionized water and anhydrous ethanol for 5 times, using an ultrasonic machine for 45 minutes each time, and obtain the filtrate by filtration and separation, and then transfer the filtrate to a vacuum drying oven for drying for 15 hours to obtain an iron-titanium alloy powder.

[0039] The anode electrode in this embodiment can also be a SnO2 anode, a TiB2-based, or a RuO2*TiO2 inert electrode in addition to a NiFe2O4-based electrode, and the cathode electrode material can also be stainless steel or molybdenum.

[0040] Example 3

[0041] This embodiment includes the following steps:

[0042] Step 1: 2.0 g of Na2FeO4 and 1.0 g of Na2Ti3O7 powder with a particle size not greater than 0.074 μm, 200 g of CaCl2-NaCl eutectic salt (wherein the molar ratio of CaCl2 to NaCl is 0.53:0.47), and 5.0 g of CaO active component are mixed uniformly and placed in a crucible, and then placed in a drying oven at a temperature of 120° C. for 12 hours to obtain anhydrous furnace charge;

[0043] Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tube resistance furnace, heat to 850°C in an inert atmosphere and keep warm for 30 minutes. After the charge is melted into a liquid melt, slowly move the nickel cathode electrode and the TiB2-based anode electrode from the top of the vertical tube resistance furnace to below the liquid surface of the molten salt system and fix them. Set the voltage between the nickel cathode electrode and the NiFe2O4-based anode electrode to 2.5V. After continuous electrolysis for 7 hours, lift each electrode from the liquid surface of the molten salt system and slowly drop to room temperature as the furnace temperature drops.

[0044] Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2 is completed, and then soak and wash it alternately with deionized water and anhydrous ethanol for 3 times, each washing is performed using an ultrasonic machine for 30 minutes, and the filtrate is obtained by filtration and separation, and then the filtrate is transferred to a vacuum drying oven for drying for 12 hours to obtain an iron-titanium alloy powder.

[0045] The anode electrode in this embodiment can also be a NiFe2O4-based, SnO2-based, RuO2*TiO2 inert electrode in addition to the TiB2-based electrode, and the cathode electrode material can also be stainless steel or molybdenum.

[0046] Example 4

[0047] This embodiment includes the following steps:

[0048] Step 1: 3.5 g of FeTiO3 powder with a particle size not greater than 0.074 μm, 200 g of Na2CO3, K2CO3, Li2CO3 eutectic salt (wherein the molar ratio of Na2CO3, Li2CO3 and K2CO3 is 0.315:0.435:0.25), and 3.0 g of Li2O active component are mixed uniformly and placed in a crucible, and then placed in a drying oven at a temperature of 100° C. for 12 hours to obtain anhydrous furnace charge;

[0049] Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tube resistance furnace, heat to 450°C in an inert atmosphere and keep warm for 30 minutes. After the charge is melted into a liquid melt, slowly move the nickel cathode electrode and the TiB2-based anode electrode from the top of the vertical tube resistance furnace to below the liquid surface of the molten salt system and fix them. Set the voltage between the nickel cathode electrode and the NiFe2O4-based anode electrode to 3.5V. After continuous electrolysis for 8 hours, lift each electrode from the liquid surface of the molten salt system and slowly drop to room temperature as the furnace temperature drops.

[0050] Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2, and then soak and wash it alternately with deionized water and anhydrous ethanol for 5 times, using an ultrasonic machine for 60 minutes each time, and obtain the filtrate by filtration and separation, and then transfer the filtrate to a vacuum drying oven for drying for 12 hours to obtain an iron-titanium alloy powder.

[0051] The anode electrode in this embodiment can also be a NiFe2O4-based, SnO2-based, RuO2*TiO2 inert electrode in addition to the TiB2-based electrode, and the cathode electrode material can also be stainless steel or molybdenum.

[0052] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A molten salt electrochemical preparation method of iron-titanium alloy powder, It is characterized in that The method comprises the following steps: Step 1: Place the mixture of iron- and titanium-containing raw material powders, alkali metal and / or alkaline earth metal inorganic salts, and active components in a crucible, and then place it in a constant temperature drying oven for drying to obtain anhydrous furnace charge; the drying temperature is not less than 100° C., and the drying time is not less than 10 hours; Step 2: Transfer the anhydrous charge obtained in step 1 to a vertical tubular resistance furnace, heat it to the electrolysis temperature under an inert atmosphere and keep it warm. After the charge is melted into a liquid melt, slowly move the cathode electrode and the anode electrode from the top of the vertical tubular resistance furnace to below the liquid surface of the molten salt system and fix them. Set a voltage of 1.0V to 5.0V between the cathode electrode and the anode electrode. After continuous electrolysis for a period of time, lift each electrode from the liquid surface of the molten salt system and slowly cool it to room temperature as the furnace temperature decreases. The electrolysis temperature is 400°C to 1000°C, and the insulation time before the cathode electrode and the anode electrode are moved to below the liquid surface of the molten salt system is 10min to 30min. Step 3: peel off the product attached to the cathode electrode after the electrolysis in step 2 is completed, and then soak and wash it alternately with deionized water and anhydrous ethanol for at least 3 times, each washing is performed using an ultrasonic machine for not less than 30 minutes, and the filtrate is obtained by filtration and separation, and the filtrate is transferred to a vacuum drying oven for drying to obtain an iron-titanium alloy powder.

2. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that The iron- and titanium-containing raw material powders in step 1 are FeO, Fe 2 O 3 、TiO 2 、FeTiO 3 、Na 2 Ti 3 O 7 MgTiO 3 、Na 2 FeO 4 、CaTiO 3 One or a combination of two or more of the above, and all contain iron and titanium elements, and the particle size of the iron- and titanium-containing raw material powder is not greater than 0.074 μm.

3. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 2, It is characterized in that When the iron-containing and titanium-containing raw material powders are two different substances, the mass ratio of the iron-containing raw material powder to the titanium-containing raw material powder is 0.5-2.0:

1.

4. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that In terms of mass fraction, the total amount of iron and titanium raw material powder added to the mixture in step 1 does not exceed 10%.

5. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that The alkali metal or / and alkaline earth metal inorganic salt in step 1 is LiCl, NaCl, KCl, CsCl, CaCl 2 MgCl 2 、BaCl 2 、Na 2 CO 3 , Li 2 CO 3 , K 2 CO 3 , Cs 2 CO 3 and BaCO 3 One or more of the following.

6. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that The active component in step 1 is Li 2 O, CaO and BaO, and the amount of the active component added to the mixture does not exceed 10% of the mass of the alkali metal or / and alkaline earth metal inorganic salt.

7. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that The anode electrode in step 2 is NiFe 2 O 4 Base, TiB 2 Base, SnO 2 or RuO 2 *TiO 2 Inert electrode, the cathode electrode is made of nickel, molybdenum or stainless steel.

8. The molten salt electrochemical preparation method of an iron-titanium alloy powder according to claim 1, It is characterized in that The electrolysis temperature in step 2 is 450° C. to 900° C., the voltage between the cathode and anode electrodes is 2.0 V to 3.5 V, and the electrolysis time is not less than 5 hours.