High-performance liquid crystal polyarylester fiber material and preparation method thereof

By mechanically cutting and crushing the liquid crystal polyaryl fibers and mixing them uniformly with MXene in acetic acid solution, a high-performance liquid crystal polyaryl fiber composite film is formed, which solves the problem of insufficient performance of traditional electromagnetic shielding materials and achieves excellent photo-thermal conversion and The electromagnetic interference shielding performance ensures the environmental protection and safety of the process.

CN118932703AActive Publication Date: 2024-11-12DONGHUA UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411221210.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Traditional metal electromagnetic shielding materials have poor corrosion resistance, high density and low electromagnetic wave absorption rate. The use of high conductivity and high thermal conductivity fillers in polymer materials is limited, especially the research on the enhancement of liquid crystal polyaryl properties as fillers is rarely conducted.

Method used

Liquid crystal polyaryl microfibers were obtained by mechanical shearing and crushing, and mixed with MXene in acetic acid solution, and then formed by suction filtration and hot pressing to form a composite film equivalent to the thickness of A4 paper, and the uniform distribution of MXene was promoted by aminocaproic acid. .

Benefits of technology

The composite film has achieved excellent photothermal conversion performance, high conductivity and good electromagnetic interference shielding performance. At the same time, the process is simple and environmentally friendly, no toxic solvent is used, and the composite film structure is tightly prevented from absorbing water and reducing shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a high-performance liquid crystal polyarylester fiber material and a preparation method thereof, the preparation method comprises the processes of preparation of a modified material, acquisition of the liquid crystal polyarylester fiber material, preparation of a fiber composite membrane and the like, and in the processes, a functional inorganic material is introduced, so that the performance of the liquid crystal polyarylester fiber is improved. The method is simple in process, safe and environment-friendly, and the functional inorganic material can be uniformly distributed on the liquid crystal polyarylester microfiber and is not easy to fall off, so that the liquid crystal polyarylester fiber with good performance is obtained, and the liquid crystal polyarylester fiber is more widely applied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high molecular polymers and relates to a high-performance liquid crystal polyarylate fiber material and a preparation method thereof. Background Art

[0002] With the development of miniaturization and high frequency of electronic products, the electromagnetic radiation problem in the operation of electronic components is becoming increasingly serious, which not only affects the working performance of nearby precision devices, but also threatens human health. Traditional metal electromagnetic shielding materials are widely used, but face problems such as poor corrosion resistance, high density and low electromagnetic wave absorption rate. Polymer materials are increasingly attracting attention due to their light weight, easy processing and excellent corrosion resistance. However, most polymers are poor conductors. Therefore, incorporating high conductivity and high thermal conductivity fillers into the polymer matrix is ​​considered to be one of the most feasible and effective methods. Liquid crystal polyarylate refers to a polymer material that can form a liquid crystal state under certain conditions. It has good thermal stability, chemical corrosion resistance and excellent mechanical properties. These excellent properties are derived from the unique structure of the mesocrystal unit in the liquid crystal polyarylate molecule, which can induce the ordering of the liquid crystal phase in the melt. At the same time, MXene is a new type of two-dimensional material. Compared with other two-dimensional materials, it has many advantages such as high specific surface area, superior conductivity, chemically active surface and strong electromagnetic wave absorption. However, few studies have focused on MXene as a filler to enhance the performance of liquid crystal polyarylate.

[0003] High-performance liquid crystal polyarylate fiber material refers to liquid crystal polyarylate fibers that are mechanically sheared and crushed into micron-sized microfibers, dispersed in acetic acid, and added with aminocaproic acid solution. After being fully mixed with MXene solution, the fibers are filtered and hot-pressed into a film with the thickness of A4 paper. The composite film formed by uniformly mixing MXene and liquid crystal polyarylate has excellent light-to-heat conversion performance, high conductivity, and good electromagnetic interference shielding performance. This high-performance liquid crystal polyarylate fiber material has not been reported. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance liquid crystal polyarylate fiber material. Micron-sized liquid crystal polyarylate microfibers are obtained by mechanical shearing and crushing, and then uniformly mixed with MXene in an acetic acid solution, filtered and hot-pressed into a film with a thickness equivalent to that of A4 paper. The composite film has excellent photothermal conversion performance, high conductivity and electromagnetic shielding performance.

[0005] In order to achieve the above object, the present invention provides a preparation method of a high-performance liquid crystal polyarylate fiber material:

[0006] (1) Slowly add Ti3AlC2 powder into a mixed solution containing lithium fluoride and hydrochloric acid and stir continuously. After etching, wash repeatedly with deionized water and centrifuge to obtain MXene;

[0007] (2) placing the liquid crystal polyarylate chopped fibers into a mechanical crusher, pouring deionized water into the crusher, and mechanically shearing and crushing the fibers to obtain a liquid crystal polyarylate microfiber aqueous dispersion, which is then filtered and dried for later use;

[0008] (3) The liquid crystal polyarylate microfibers in step (2) are added to a beaker containing acetic acid, and then uniformly dispersed using a digital high-speed dispersing homogenizer, and the aminocaproic acid solution is added. After continuous stirring, the MXene solution is slowly added dropwise, and the suspension is filtered to form a film, dried, and hot-pressed.

[0009] Preferably, the mass ratio of the Ti3AlC2 powder to lithium fluoride in step (1) is (0.6-0.7): 1, 1 g of lithium fluoride corresponds to 12-13 mL of 9 mol / mL hydrochloric acid solution, stirred at 200-400 rpm for 24-48 h at 30-40 ° C. After etching, it is repeatedly washed with deionized water to a pH value of 6.0-7.0, and then centrifuged at 3000-4000 rpm for 20-40 min to obtain MXene.

[0010] Preferably, the liquid crystal polyarylate chopped fibers in step (2) have a length of 2 to 4 cm and a diameter of 30 to 40 μm, 10 g of the chopped fibers correspond to 2 to 4 L of deionized water, the mechanical shearing and crushing time is 1 h to 2 h, and the obtained microfiber diameter range is 0.5 to 3 μm. The obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50 to 70 ° C and dried for 4 to 6 hours.

[0011] Preferably, 100 mg of the liquid crystal polyarylate microfibers described in step (3) are added to a beaker containing 15 to 30 mL of acetic acid, the speed of the digital high-speed dispersing homogenizer is 4 to 5 kr / min, 2 to 3 mL of 20 mg / mL aminocaproic acid solution is added, and the mixture is stirred at a speed of 200 to 400 rpm for 24 to 48 h. During the stirring process, 10 to 15 mg / mL of MXene solution is slowly added dropwise, and the suspension is filtered to form a film. The vacuum oven drying temperature is 40 to 50 ° C, the drying time is 3 to 4 h, the hot pressing temperature is 25 ° C, 220 ° C, 240 ° C, 260 ° C and 280 ° C, and the hot pressing pressure is 5 to 10 MPa.

[0012] Compared with the prior art, the present invention has the following positive and beneficial effects:

[0013] (1) The present invention provides a method for preparing a high-performance liquid crystal polyarylate fiber material. The preparation process is simple. Liquid crystal polyarylate fibers are mechanically sheared and crushed to obtain liquid crystal polyarylate microfibers. No chemical reagents are added in the process, and only deionized water is used. The processing process is safe and environmentally friendly. The mixing process of liquid crystal polyarylate microfibers and MXene does not require the participation of toxic reagent solvents, nor does it emit toxic gases / liquids. Only acetic acid is used as a solvent, and the acetic acid after filtration can be reused, which is pollution-free to the environment.

[0014] (2) The present invention provides a method for preparing a high-performance liquid crystal polyarylate fiber material. The MXene and liquid crystal polyarylate microfibers are evenly mixed thanks to the action of aminocaproic acid. After continuous stirring, the MXene flakes are evenly distributed on the surface of the liquid crystal polyarylate microfibers, so that the composite film has good photothermal conversion performance, electrical conductivity and electromagnetic shielding effectiveness.

[0015] (3) The present invention provides a method for preparing a high-performance liquid crystal polyarylate fiber material. The composite film formed by MXene and liquid crystal polyarylate microfibers has a thickness equivalent to that of A4 paper after hot pressing. Its internal structure is more compact and has better hydrophobicity, which can prevent the shielding performance of the composite film from being reduced due to water absorption, thereby forming a more excellent environmental stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 (a) is a macroscopic photograph of liquid crystal polyarylate microfibers. Figure 1 (b) is a macroscopic photograph of liquid crystal polyarylate microfibers dispersed in deionized water and acetic acid solution.

[0017] Figure 2 (a) is the SEM morphology of liquid crystal polyarylate fiber. Figure 2 (b) is the SEM morphology of liquid crystal polyarylate microfibers.

[0018] Figure 3 (a) is a macroscopic photograph of pure liquid crystal polyarylate microfiber membrane. Figure 3 (b) is a macroscopic photograph of the MXene / liquid crystal polyarylate microfiber composite membrane. Figure 3 (c) Macroscopic photograph of pure liquid crystal polyarylate microfiber membrane after hot pressing at 25℃ and 10MPa. Figure 3 (d) Macroscopic photograph of the MXene / liquid crystal polyarylate microfiber composite film after hot pressing at 260°C and 10 MPa.

[0019] Figure 4 (a) is the EMI SE of MXene / liquid crystal polyarylate microfiber composite membrane, Figure 4 (b) Shielding efficiency of MXene / liquid crystal polyarylate microfiber composite film.

[0020] Figure 5The electrical conductivity of the MXene / liquid crystal polyarylate microfiber composite film after hot pressing at 25°C and 10MPa.

[0021] Figure 6 The electrical conductivity of the MXene / liquid crystal polyarylate microfiber composite film after hot pressing at 260°C and 10MPa.

[0022] Comparative Example 1

[0023] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0024] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0025] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of deionized water. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 1.8 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0026] Comparative Example 2

[0027] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0028] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0029] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of deionized water. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 4.3 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0030] Comparative Example 3

[0031] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0032] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0033] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of deionized water. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, slowly add 10 mL of 10 mg / mL MXene solution, filter the suspension into a membrane, and put it into a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0034] Example 1

[0035] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0036] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0037] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 1.8 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0038] Example 2

[0039] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0040] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0041] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 4.3 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0042] Example 3

[0043] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0044] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0045] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, slowly add 10 mL of 10 mg / mL MXene solution, filter the suspension into a membrane, and put it into a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 25°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0046] Example 4

[0047] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0048] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0049] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 1.8 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 240°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0050] Example 5

[0051] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0052] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0053] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 4.3 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 240°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0054] Example 6

[0055] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0056] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0057] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, slowly add 10 mL of 10 mg / mL MXene solution, filter the suspension into a film, and put it into a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 240°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite film into a thickness equivalent to A4 paper.

[0058] Example 7

[0059] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0060] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0061] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 1.8 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 260°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0062] Example 8

[0063] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0064] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0065] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, 4.3 mL of 10 mg / mL MXene solution is slowly added dropwise, the suspension is filtered to form a membrane, and placed in a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 260°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0066] Example 9

[0067] 0.3 g Ti3AlC2 powder was slowly added to a mixed solution containing 0.48 g lithium fluoride and 6 mL 9 mol / mL hydrochloric acid, and stirred at 300 rpm for 36 h at 35 °C. After etching, it was repeatedly washed with deionized water until the pH value was 6.0-7.0, shaken by the robotic arm for 1 h, ultrasonicated for 15 min, and then centrifuged at 3500 rpm for 30 min to obtain a MXene solution.

[0068] Use a cutter to cut the liquid crystal polyarylate fibers into 2 cm short fibers with a diameter of 30-40 μm, put them into a mechanical crusher, add 3 L of deionized water, and mechanically shear and crush for 1 hour. After physical disassembly, the obtained liquid crystal polyarylate microfiber aqueous dispersion is filtered and placed in a vacuum oven at 50°C for drying for 5 hours.

[0069] Take 100 mg of liquid crystal polyarylate microfibers and add them to a beaker containing 20 mL of acetic acid. Use a digital high-speed disperser to break up the liquid crystal polyarylate microfibers at a speed of 5 kr / min, then add 2.5 mL of 20 mg / mL aminocaproic acid solution, and stir at 300 rpm for 48 hours. During the stirring process, slowly add 10 mL of 10 mg / mL MXene solution, filter the suspension into a membrane, and put it into a vacuum oven at 50°C for 4 hours. Use a flat vulcanizer at 260°C and a pressure of 10 MPa to press the MXene / liquid crystal polyarylate microfiber composite membrane into a thickness equivalent to A4 paper.

[0070] Therefore, compared with the control example, replacing deionized water with acetic acid solution as the solvent effectively solved the uniformity problem of the MXene / liquid crystal polyarylate composite film. Because water is used as a solvent, there is no interaction force between MXene and liquid crystal polyarylate microfibers. The size of MXene is 3 to 5 μm. During the filtration process, the MXene flakes will be filtered off first, which will greatly affect the performance of the composite film. Using acetic acid as a solvent, under acidic conditions, coupled with the effect of aminocaproic acid, MXene can be evenly dispersed on the surface of liquid crystal polyarylate microfibers. After filtration and hot pressing, the formed MXene / liquid crystal polyarylate composite film has excellent light-to-heat conversion performance, high conductivity and good electromagnetic interference shielding effectiveness.

[0071] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

[0072] Table 1 Parameters and experimental results of control examples and various examples

[0073]

Claims

1. A high-performance liquid crystal polyarylate fiber material and a preparation method thereof, characterized in that: The steps are as follows: (1) Slowly add Ti3AlC2 powder into a mixed solution containing lithium fluoride and hydrochloric acid and stir continuously. After etching, wash repeatedly with deionized water and centrifuge to obtain MXene; (2) placing the liquid crystal polyarylate chopped fibers into a mechanical crusher, pouring deionized water into the crusher, and mechanically shearing and crushing the fibers to obtain a liquid crystal polyarylate microfiber aqueous dispersion, which is then filtered and dried for later use; (3) The liquid crystal polyarylate microfibers in step (2) are added to a beaker containing acetic acid, and then uniformly dispersed using a digital high-speed dispersing homogenizer, and the aminocaproic acid solution is added. After continuous stirring, the MXene solution is slowly added dropwise, and the suspension is filtered to form a film, dried, and hot-pressed.

2. A high performance liquid crystal polyarylate fiber material and a preparation method thereof according to claim 1, characterized in that: The mass ratio of Ti3AlC2 powder to lithium fluoride in step (1) is (0.6-0.7): 1, 1 g of lithium fluoride corresponds to 12-13 mL of 9 mol / mL hydrochloric acid solution, stirred at 200-400 rpm for 24-48 h at 30-40 ° C. After etching, it is repeatedly washed with deionized water to a pH value of 6.0-7.0, and then centrifuged at 3000-4000 rpm for 20-40 min to obtain MXene.

3. A high performance liquid crystal polyarylate fiber material and a preparation method thereof according to claim 1, characterized in that: The liquid crystal polyarylate chopped fibers described in step (2) have a length of 2 to 4 cm and a diameter of 30 to 40 μm. 10 g of chopped fibers correspond to 2 to 4 L of deionized water. The mechanical shearing and crushing time is 1 to 2 hours. The diameter of the obtained microfibers ranges from 0.5 to 3 μm.

4. A high performance liquid crystal polyarylate fiber material and a preparation method thereof according to claim 1, characterized in that: 100 mg of the liquid crystal polyarylate microfibers described in step (3) are added to a beaker containing 15 to 30 mL of acetic acid, the speed of the digital high-speed dispersing homogenizer is 4 to 5 kr / min, 2 to 3 mL of 20 mg / mL aminocaproic acid solution is added, and the mixture is stirred at a speed of 200 to 400 rpm for 24 to 48 h. During the stirring process, 10 to 15 mg / mL of MXene solution is slowly added dropwise, and the suspension is filtered to form a film. The vacuum oven drying temperature is 40 to 50 ° C, the drying time is 3 to 4 h, the hot pressing temperature is 25 ° C, 220 ° C, 240 ° C, 260 ° C and 280 ° C, and the hot pressing pressure is 5 to 10 MPa.

5. A high-performance liquid crystal polyarylate fiber material and a preparation method thereof, characterized in that The high performance liquid crystal polyarylate fiber is prepared by the preparation method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Method for making electromagnetic shielding fabric based on two-dimensional layered MXene nanosheets and product

    CN109868646A

  • MXene hollow fiber and preparation method thereof

    CN118345527A

  • MXene coated fiber and preparation method thereof

    CN118374969A

  • Method for preparing high-conductivity flexible liquid crystal polyarylester nanofiber membrane by in-situ self-assembly method

    CN118516850A

  • High-strength polyarylate fiber

    JP2004107826A