Sizing large-tow carbon fiber for rubber-based composite material and preparation method thereof

By using a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide and a step-by-step sizing process, the interface bonding ability between sizing large tow carbon fiber and rubber matrix is ​​significantly improved, and the problem of poor adhesion in the prior art is solved, so as to achieve The industrial production of high-performance rubber-based composite materials.

CN118932719APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310536591.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the bonding force between the sizing large tow carbon fiber and the rubber matrix is ​​poor, resulting in poor mechanical properties of the prepared rubber matrix composite materials, complex processes and high costs, making it difficult to achieve large-scale industrial production.

Method used

Using a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide, through a step-by-step sizing process, combined with infrared radiation drying and electric heating hot roll drying, the interface bonding ability between carbon fiber and rubber matrix is ​​significantly improved and mechanical properties are improved.

Benefits of technology

The interface bonding capability between sizing large tow carbon fiber and rubber matrix is ​​significantly improved. The compression strength after impact reaches more than 400MPa and the adhesion force is not less than 150N. It is suitable for existing carbon fiber industrial production lines, with low cost and suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226498710000101
    Figure BDA0004226498710000101
  • Figure BDA0004226498710000111
    Figure BDA0004226498710000111
  • Figure BDA0004226498710000112
    Figure BDA0004226498710000112
Patent Text Reader

Abstract

The invention relates to the technical field of sizing large-tow carbon fiber preparation, in particular to sizing large-tow carbon fiber for a rubber-based composite material and a preparation method of the sizing large-tow carbon fiber, and discloses the sizing large-tow carbon fiber for the rubber-based composite material and the preparation method of the sizing large-tow carbon fiber. The method comprises the following steps: performing pre-oxidation, low-temperature carbonization, high-temperature carbonization, surface treatment, water washing, sizing and drying, and winding and collecting the polyacrylonitrile-based precursor; the sizing and drying comprises the following steps: pre-sizing and pre-drying the washed carbon fibers by adopting a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide, and then carrying out secondary sizing and secondary drying on the initial carbon fibers by adopting resorcinol formaldehyde latex; the contact angle of the pre-sizing agent is not more than 55 degrees, and the surface tension is not more than 55 mN / m. The pre-drying is infrared radiation drying, and the secondary drying sequentially comprises electric heating hot roller drying and horizontal hot air drying. The basic mechanical property of the sizing large-tow carbon fiber-rubber-based composite material is met, and meanwhile, the binding power of the sizing large-tow carbon fiber and the rubber matrix is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sized large-tow carbon fiber preparation, and in particular to a sized large-tow carbon fiber for a rubber-based composite material and a preparation method thereof. Background Art

[0002] Rubber-based composite materials are advanced functional structural composite materials with unique properties, especially carbon fiber reinforced resin-based composite materials, which can combine the high specific strength, high modulus, high thermal conductivity, chemical corrosion resistance of carbon fiber and the high toughness and high elasticity of rubber matrix. However, most carbon fibers have an inert surface, and the two-phase interface properties with the rubber matrix are very different, so it is difficult to effectively combine them into a solid integrated material, resulting in poor load transfer, and the fiber cannot effectively play its reinforcing role, and the mechanical strength, toughness and other properties of the product are affected.

[0003] CN111484654A discloses a heat-conducting rubber material, which first treats carbon fiber with a silane coupling agent and then uses CO 2 Plasma etching treatment, combined with pre-treated hexagonal boron nitride powder and pre-treated nano powder, can improve the thermal conductivity and mechanical properties of rubber materials. This solution can improve the interface bonding between carbon fiber and rubber materials to a certain extent, but the treatment process is complicated, the industrialization level of plasma etching is low, continuous production is not possible, the cost of the formula powder is high, and it is difficult to apply on an online scale.

[0004] CN103265763A applied for a modified carbon fiber EPDM rubber cable sheath material and its preparation method. The strength of the cable sheath material can be greatly improved by microwave and ultrasonic modification of the reinforcing agent carbon fiber, but the required equipment is expensive and the process is complicated, which is not suitable for industrial-scale production and application. In addition, the above schemes cannot achieve good sizing of large-tow carbon fibers of 240K and above, which leads to poor mechanical properties of the large-tow carbon fibers after sizing. At the same time, when applied to rubber materials, the bonding force between the carbon fibers and the rubber matrix is ​​poor. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems in the prior art that the bonding force between sized large-tow carbon fibers and a rubber matrix is ​​poor, and that the mechanical properties of a rubber-based composite material prepared from the sized large-tow carbon fibers are poor. A sized large-tow carbon fiber for a rubber-based composite material and a preparation method thereof are provided. The method has low operating costs and can significantly improve the interface bonding ability between the sized large-tow carbon fibers and the rubber matrix while satisfying the basic mechanical properties of the sized large-tow carbon fiber-rubber-based composite material prepared from the sized large-tow carbon fibers by using a step-by-step sizing method combined with a specific pre-sizing agent.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing sized large-tow carbon fiber for rubber-based composite materials, the method comprising: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sized large-tow carbon fiber;

[0007] The sizing and drying comprises the following steps:

[0008] Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide to obtain initial carbon fiber;

[0009] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0010] Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤55mN / m;

[0011] The pre-drying method is infrared radiation drying;

[0012] The secondary drying step includes: electrically heated hot roller drying and horizontal hot air drying in sequence.

[0013] The second aspect of the present invention provides a sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0014] Through the above technical scheme, the sized large-tow carbon fiber for rubber-based composite materials and the preparation method thereof provided by the present invention achieve the following beneficial effects:

[0015] (1) The present invention introduces aromatic polyamide into the pre-sizing agent, which can significantly improve the subsequent RFL emulsion and carbon fiber two-phase interface wetting and spreading, and effectively alleviate the stress concentration of the multi-interface phase after thermal curing, and effectively improve the mechanical properties of the prepared sized large-tow carbon fiber-rubber-based composite material. Specifically, the post-impact compressive strength can reach more than 400 MPa; and the interface bonding ability between the sized large-tow carbon fiber and the rubber matrix is ​​further improved, and the bonding force is not less than 150N.

[0016] (2) The present invention selects a specific pre-sizing agent with a contact angle of ≤55° and a surface tension of ≤55mN / m, and uses it in combination with the RFL emulsion, and combines the process of "pre-sizing-pre-drying-secondary sizing-secondary drying". The pre-drying adopts an infrared radiation drying method, and the secondary drying adopts an electric heating hot roller and a horizontal hot air dryer in sequence. The production process can significantly improve the interface bonding ability between the sized large-tow carbon fiber and the rubber matrix.

[0017] (3) The method of the present invention is applicable to the existing carbon fiber industrial production line, does not require much modification and upgrading, and has strong process adaptability; the sizing agent components and RFL emulsion used are low-cost and have broad industrial application prospects. DETAILED DESCRIPTION

[0018] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0019] The first aspect of the present invention provides a method for preparing sized large-tow carbon fibers for rubber-based composite materials, the method comprising: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding polyacrylonitrile-based precursor fibers to obtain the sized large-tow carbon fibers;

[0020] The sizing and drying comprises the following steps:

[0021] Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide to obtain initial carbon fiber;

[0022] Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber;

[0023] Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤55mN / m;

[0024] The pre-drying method is infrared radiation drying;

[0025] The secondary drying step includes: electrically heated hot roller drying and horizontal hot air drying in sequence.

[0026] In the present invention, the inventors have found that in the process of sizing carbon fiber, a layer of hydrophilic pre-sizing agent is coated on the surface of the carbon fiber, and then RFL emulsion is coated after drying, which can improve the bonding ability between the sized large-tow carbon fiber and the rubber matrix. However, arbitrarily selecting a hydrophilic pre-sizing agent cannot achieve a good coupling effect with the RFL emulsion. For the pre-sizing agent described in the present invention, only when its contact angle is ≤55° and the surface tension is ≤55mN / m, can the subsequent RFL emulsion achieve secondary uniform infiltration on the carbon fiber surface, thereby having a good coupling effect. At the same time, the introduction of aromatic polyamide in the pre-sizing agent can significantly improve the interfacial bonding ability between the sized large-tow carbon fiber and the rubber matrix and improve the mechanical properties of the sized large-tow carbon fiber-rubber-based composite material.

[0027] In the present invention, the pre-oxidation is carried out in an oxidation furnace with multiple heating temperature zones. Exemplarily, the present invention is carried out in an oxidation furnace with 4 heating temperature zones. The temperatures of the 4 heating temperature zones are respectively set to 0-250°C, 0-300°C, 0-300°C and 0-350°C. The total pre-oxidation time is 30-80min. The pre-oxidation time of each temperature zone is ensured to be the same. The stretching ratios in the oxidation furnace with the 4 heating temperature zones are 0-1.8, 0.8-1, 0.8-1 and 0.8-1, respectively.

[0028] In the present invention, the temperatures of the four heating zones, the total time of pre-oxidation and the drawing ratio are controlled to meet the above ranges, thereby achieving efficient and rapid pre-oxidation.

[0029] In the present invention, the low-temperature carbonization is carried out in an oxidation furnace with multiple heating temperature zones. Exemplarily, the present invention is preferably carried out in a low-temperature carbonization furnace with 5 heating temperature zones, and the temperatures of the 5 heating temperature zones are respectively set to 0-700°C, 0-700°C, 0-800°C, 0-950°C and 0-950°C. When the pre-oxidized filament bundle is run in the low-temperature carbonization furnace, the draft ratio is controlled to be 1-1.2, and the total residence time in the low-temperature carbonization furnace is 1-10 minutes to obtain low-temperature carbonized filaments.

[0030] In the present invention, the high-temperature carbonization process is carried out in an oxidation furnace with multiple heating temperature zones. Exemplarily, the present invention is preferably carried out in a high-temperature carbonization furnace with 5 heating temperature zones, and the temperatures of the 5 heating temperature zones are 0-1300° C., 0-1400° C., 0-1700° C., 0-1900° C. and 0-2200° C. When the tow runs in the high-temperature carbonization furnace, the draft ratio is controlled to be 0.6-0.95, and the total residence time in the high-temperature carbonization furnace is 1-10 min to obtain high-temperature carbonized filaments.

[0031] In the present invention, the surface treatment conditions include: using ammonium bicarbonate aqueous solution as electrolyte, voltage of 15-25V, electrolyte concentration of 10-30wt%, and treatment time of 50-80 seconds.

[0032] In the present invention, the water washing conditions include: washing at 40-60°C and a water flow rate of 2500-6500 L / h.

[0033] In the present invention, the winding and collecting can be carried out under a tension of 2500-3500 cN.

[0034] In the present invention, the term "large tow" refers to a large tow carbon fiber with more than 48,000 carbon fibers per bundle (abbreviated as 48K). According to a specific embodiment of the present invention, the large tow carbon fiber described in the present invention is 240K, that is, the number of carbon fibers per bundle is 240,000.

[0035] In the present invention, the preparation method of the pre-sizing agent can adopt the preparation method of the common emulsion in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0036] In the present invention, the surface tension refers to the surface tension when the material is diluted with water to a concentration of 2 wt %.

[0037] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber emulsion is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0038] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0039] According to the present invention, the contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤50 mN / m.

[0040] According to the present invention, the average particle size of the aromatic polyamide is ≤1 micron.

[0041] In the present invention, the average particle size of the aromatic polyamide meets the above range, which can ensure that the pre-sizing agent is infiltrated and spread on the surface of the carbon fiber, thereby improving the two-phase coupling effect.

[0042] Furthermore, the average particle size of the aromatic polyamide is ≤0.5 micrometer.

[0043] According to the present invention, the mass ratio of the polyvinyl alcohol to the aromatic polyamide is 1:0.3-0.8.

[0044] In the present invention, when the mass ratio of the polyvinyl alcohol to the aromatic polyamide satisfies the above range, the bonding force between the sized large tow carbon fiber and the rubber matrix can be significantly improved while effectively improving the mechanical properties of the sized large tow carbon fiber-rubber composite material.

[0045] Furthermore, the mass ratio of the polyvinyl alcohol to the aromatic polyamide is 1:0.4-0.6.

[0046] In the present invention, the polyvinyl alcohol can be polyvinyl alcohol with different alcoholysis degrees, preferably partially alcoholysed polyvinyl alcohol.

[0047] According to the present invention, the alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%.

[0048] According to the present invention, the number average molecular weight of the polyvinyl alcohol is 20,000-200,000 g / mol, preferably 50,000-150,000 g / mol.

[0049] According to the present invention, the number average molecular weight of the aromatic polyamide is 5000-35000 g / mol, preferably 10000-20000 g / mol.

[0050] According to the present invention, the aromatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid.

[0051] In the present invention, “the aromatic polyamide includes a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid” means that the aromatic polyamide is prepared by condensation polymerization of a diamine and an aromatic dibasic acid.

[0052] In the present invention, the diamine can be commercially available, for example, it can be at least one of ethylenediamine, m-phenylenediamine, p-phenylenediamine, hexamethylenediamine, and decanediamine.

[0053] In the present invention, the aromatic dibasic acid can be commercially available, for example, phthalic acid, isophthalic acid, and terephthalic acid.

[0054] In the present invention, compared with aliphatic polyamide, when the aromatic polyamide is added to the pre-sizing agent and used in combination with the RFL emulsion, the bonding force between the sized large-tow carbon fiber and the rubber matrix can be further improved.

[0055] According to the present invention, the molar ratio of the structural unit A to the structural unit B is 1-2:1.

[0056] In the present invention, the aromatic polyamide can be commercially available, such as RI925, RI930, etc.

[0057] According to the present invention, the pre-drying temperature is 60-100°C, preferably 70-90°C.

[0058] According to the present invention, in step 2, the temperature of the electrically heated hot roller drying is 80-230°C, preferably 100-180°C;

[0059] According to the present invention, the temperature of the horizontal hot air drying is 90-240°C, preferably 110-190°C.

[0060] In the present invention, the infrared radiation drying can be performed using an infrared radiation drying machine, and the infrared radiation heating drying machine contains a carbon medium-wave infrared radiator.

[0061] In the present invention, when infrared radiation drying is performed, the distance between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber is 40-80 mm, and the power density is 20-50 kW / m 2 .

[0062] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

[0063] According to the present invention, based on the mass of the washed carbon fiber tow, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%.

[0064] According to the present invention, based on the mass of the washed carbon fiber tow, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

[0065] In the present invention, the prepared sized large-tow carbon fiber can be used in a reinforced rubber composite material, wherein the content of the sized large-tow carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0066] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0067] In the present invention, there is no particular limitation on the type of the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, butyl rubber, etc., preferably the same type as the rubber emulsion in the RFL emulsion.

[0068] The second aspect of the present invention provides a sized large-tow carbon fiber prepared by the preparation method described in the first aspect of the present invention.

[0069] The present invention will be described in detail below by way of examples. In the following examples, each parameter is obtained by the following method.

[0070] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0071] Surface tension: The pre-sizing agent was diluted to a concentration of 2 wt % and the surface tension was tested using a dynamic surface tension meter at a temperature of 25°C.

[0072] Adhesion: The sized large tow carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sized large tow carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sized large tow carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out 1 cm of length is the adhesion between the fiber and the rubber.

[0073] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0074] Compression strength after impact: Referring to SACMA SRM 2R-94 standard, a 6.7 J / mm drop hammer impact is applied to the center of the sized large-tow carbon fiber-rubber composite sample to calculate the compression strength after impact.

[0075] KTM-1M epoxy emulsion, purchased from Sinopharm Reagent;

[0076] Polyvinyl alcohol (PVA) was purchased from Sinopharm.

[0077] Aromatic polyamide RI925 and RI930 were purchased from Sinopharm Reagent.

[0078] Examples 1-6

[0079] Embodiments 1-6 are methods for producing a uniform 240K carbon fiber, comprising:

[0080] Pre-oxidation: The polyacrylonitrile-based precursor passes through oxidation furnace No. 1, oxidation furnace No. 2, oxidation furnace No. 3, and oxidation furnace No. 4 for pre-oxidation treatment. The temperatures of the four heating temperature zones are 238°C, 246°C, 256°C, and 268°C, respectively. The pre-oxidation time in each temperature zone is the same, and the total pre-oxidation time is 44 minutes. The draft ratios between the oxidation furnaces in the four heating temperature zones are 1.28, 0.98, 0.98, and 0.97, respectively;

[0081] Low-temperature carbonization: Using nitrogen as the medium, the pre-oxidized filament bundles were sequentially passed through a low-temperature carbonization furnace with five heating temperature zones at 530°C, 640°C, 700°C, 810°C, and 860°C, respectively. The draft ratio of each zone was controlled to be 1.09, and the total residence time in the low-temperature carbonization furnace was 1.2 minutes to obtain low-temperature carbonized filaments.

[0082] High temperature carbonization: Using nitrogen as the medium, the low temperature carbonized wire passes through a high temperature carbonization furnace with five heating temperature zones at 955°C, 1260°C, 1290°C, 1350°C, and 1450°C, respectively. The draft ratio of each zone is controlled to be 0.81, and the total residence time in the high temperature carbonization furnace is 1.2 minutes to obtain high temperature carbonized wire;

[0083] Surface treatment: The high-temperature carbonized fibers are passed through a traction device into a surface treatment tank, with an ammonium bicarbonate aqueous solution as the electrolyte, a voltage of 22 V, an electrolyte concentration of 22 wt%, and a treatment time of 60 seconds to obtain surface-treated carbon fibers;

[0084] Washing: washing the surface-treated carbon fiber at a washing flow rate of 5500 L / h and a washing temperature of 55° C. to obtain a washed carbon fiber tow;

[0085] Sizing and drying: The washed carbon fiber tow is directly introduced into the first sizing tank for pre-sizing, and then passes through the infrared radiation dryer for pre-drying under the set process parameters; then enters the second sizing tank for secondary sizing, and then passes through the electric heating hot roller and the horizontal hot air dryer in turn for secondary drying under the set process parameters to obtain the sized large tow carbon fiber;

[0086] Winding and collecting: Under a tension of 2900-3120 cN, a carbon fiber winder is used to wind and collect the sized large-tow carbon fiber to obtain the sized large-tow carbon fiber.

[0087] Among them, the type of the pre-sizing agent is shown in Table 1, the properties of the pre-sizing agent, the molar ratio of resorcinol to formaldehyde in the secondary sizing agent RFL emulsion, the pre-sizing amount and the secondary sizing amount are shown in Table 2, and the pre-sizing drying and secondary sizing drying process parameters are shown in Table 3.

[0088] Comparative Example 1

[0089] Comparative Example 1 is a method for manufacturing 240K carbon fiber, which is manufactured according to the method of Example 1, except that the sizing and drying process is as follows: sizing the unsized large tow carbon fiber with a commercially available KTM-1M epoxy emulsion sizing agent, and horizontal hot air drying at a drying temperature of 100° C. Winding and collecting the filaments to prepare the sized large tow carbon fiber.

[0090] Comparative Example 2

[0091] Comparative Example 2 is a method for manufacturing 240K carbon fiber, which is based on the method of Example 1, except that the RFL emulsion in Example 2 is used to size the unsized large tow carbon fiber, and the fiber is dried in a horizontal hot air drying method at a drying temperature of 150° C. The sized large tow carbon fiber is prepared by winding and collecting the fiber.

[0092] Comparative Example 3

[0093] Comparative Example 3 is a method for manufacturing 240K carbon fiber, which is based on the method of Example 1, except that the unsized large tow carbon fiber is pre-sized with polyvinyl alcohol PVA1788 water-based sizing agent, and horizontal hot air drying is performed at a drying temperature of 80°C; then the RFL emulsion in Example 2 is used for secondary sizing at a drying temperature of 165°C. The sized large tow carbon fiber is prepared by winding and collecting.

[0094] Table 1

[0095]

[0096] Table 2

[0097] Table 3

[0098] ps: The "distance" in the table refers to the height between the carbon medium wave infrared radiator of the infrared radiation heating dryer and the carbon fiber

[0099] The sized large tow carbon fiber prepared in the embodiment and the comparative example and the rubber matrix were prepared into a sized large tow carbon fiber-rubber matrix composite material, and the adhesion test was carried out. The post-impact compression strength of the sized large tow carbon fiber-rubber composite material was tested with reference to the SACMA SRM 2R-94 standard. The results are shown in Table 4.

[0100] Table 4

[0101] Compression strength after impact (MPa) Adhesion force(N) Comparative Example 1 231 101 Comparative Example 2 216 112 Comparative Example 3 256 119 Example 1 419 157 Example 2 420 169 Example 3 427 161 Example 4 425 153 Example 5 418 166 Example 6 432 159

[0102] From the results in Table 4, it can be seen that in Comparative Example 1, only the traditional epoxy resin emulsion is used as the sizing agent, and in Comparative Example 2, only the RFL emulsion is used as the sizing agent. The prepared sized large tow carbon fiber has low bonding force with the rubber matrix and low impact resistance. The pre-sizing agent used in Comparative Example 3 contains only polyvinyl alcohol, and the surface tension is too large, so the improvement effect is not obvious.

[0103] Examples 1-6 use a pre-sizing agent containing polyvinyl alcohol to which aromatic polyamide is added and has a contact angle of ≤55° and a surface tension of ≤55mN / m in combination with an RFL emulsion, and through a specific sizing and drying process, the final prepared sized large-tow carbon fiber has excellent interfacial bonding with the rubber matrix and good impact resistance, which can meet the application requirements of higher-level rubber-based composite materials, and the overall improvement effect is obvious.

[0104] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized large-tow carbon fibers for rubber-based composite materials, characterized in that: The method comprises: pre-oxidizing, low-temperature carbonizing, high-temperature carbonizing, surface treating, washing, sizing, drying and winding the polyacrylonitrile-based precursor to obtain the sizing large-tow carbon fiber; The sizing and drying comprises the following steps: Step 1: pre-sizing and pre-drying the washed carbon fiber tow using a pre-sizing agent containing polyvinyl alcohol and aromatic polyamide to obtain initial carbon fiber; Step 2: secondary sizing and secondary drying the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing large tow carbon fiber; Wherein, the contact angle of the pre-sizing agent is ≤55° and the surface tension is ≤55mN / m; The pre-drying method is infrared radiation drying; The secondary drying step includes: electrically heated hot roller drying and horizontal hot air drying in sequence.

2. The method according to claim 1, wherein: The contact angle of the pre-sizing agent is ≤10° and the surface tension is ≤50mN / m; Preferably, the average particle size of the aromatic polyamide is ≤1 micron, preferably ≤0.5 micron.

3. The method according to claim 1 or 2, wherein: The mass ratio of the polyvinyl alcohol to the aromatic polyamide is 1:0.3-0.8, preferably 1:0.4-0.

6.

4. The method according to claim 1 or 2, wherein: The alcoholysis degree of the polyvinyl alcohol is 78-99%, preferably 88-92%; Preferably, the number average molecular weight of the polyvinyl alcohol is 20000-200000 g / mol, preferably 50000-150000 g / mol; Preferably, the number average molecular weight of the aromatic polyamide is 5000-35000 g / mol, preferably 10000-20000 g / mol.

5. The method according to claim 1 or 2, wherein: The aromatic polyamide comprises a structural unit A provided by a diamine and a structural unit B provided by an aromatic dibasic acid; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:

1.

6. The method according to claim 1 or 2, wherein: In step 1, the pre-drying temperature is 60-100°C, preferably 70-90°C.

7. The method according to claim 1 or 2, wherein: In step 2, the temperature of the electrically heated hot roller drying is 80-230°C, preferably 100-180°C; Preferably, the temperature of the horizontal hot air drying is 90-240°C, preferably 110-190°C.

8. The preparation method according to claim 1 or 2, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:3-25, preferably 1:8-18.

9. The preparation method according to claim 1 or 2, wherein: Based on the weight of the washed carbon fiber tow, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the washed carbon fiber tow, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

10. The sized large-tow carbon fiber prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Ethylene-propylene-diene-monome rubber cable sheath material made from modified carbon fibers and preparation method of sheath material

    CN103265763A

  • Heat-conducting rubber material and rubber track

    CN111484654A