Method for increasing paper pulp yield by adding amino acid
Through the three-eutectic eutectic solvent and microwave reaction technology, bamboo is pretreated, the problem of cellulose degradation of bamboo is solved, the pulp yield is improved, and an efficient and environmentally friendly pulping process is achieved, reducing reagent costs and environmental pollution are carried out. .
Patent Information
- Application Number
- CN202411214392.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-31
AI Technical Summary
In the existing pulping technology, bamboo cellulose, hemicellulose and lignin are closely combined, resulting in cellulose degradation under more severe cooking conditions, reducing the pulp yield. In addition, the mild pulping technology has environmental pollution, high reagent cost and fiber. The problem of decreasing yield rate.
The ternary eutectic solvent cooking method was used to combine microwave reactions to pretreat the bamboo material by a mixed solvent of choline chloride, amino acid and L-lactic acid to form a clear and transparent solution, and was carried out under conditions of 120℃ to 140℃. The microwave reaction was performed from 10 to 30 minutes, followed by washing to neutral using acetone solution, anhydrous ethanol and deionized water to obtain a slurry with high pulp yield.
It improves the yield of pulp, shortens the cooking time, reduces environmental pollution, reduces the cost of reagents, and protects cellulose through the addition of amino acids to prevent its degradation, achieving efficient cellulose retention.
Abstract
Description
Technical Field
[0001] The invention relates to the field of papermaking, and in particular to a pulping method for significantly improving cellulose retention rate by adding amino acids. Background Art
[0002] Among the currently developed and mature pulping processes, the pulping route using wood as the main raw material accounts for about 95%. The rapid development of the papermaking industry has brought tremendous pressure on the sustainable supply of global forest resources. While expanding the source channels of pulping and papermaking raw materials, researchers and the industry are constantly improving pulping technology to improve pulp yield and pulp quality.
[0003] my country is rich in bamboo resources. The properties of bamboo fiber are similar to those of coniferous wood. It is an excellent raw material for pulping and can replace part of wood pulp. Patent CN116145457B first pre-hydrolyzes bamboo with steam, then performs alkaline cooking, oxygen alkali bleaching, pulping and other processes to obtain bleached bamboo pulp with a yield of about 31%. Patent CN116695479A first pre-impregnates bamboo slices with warm black liquor, then replaces the warm black liquor with hot black liquor, and after the temperature reaches 125-135°C, hot white liquor with a temperature of 150°C or above is added for cooking, and the final yield is 46%-49%. In recent years, low eutectic solvents have begun to be used in the preparation of high-quality pulp. Patent CN116200959B mixes bamboo and straw in a certain proportion, and then uses a low eutectic solvent composed of choline chloride and DL-menthol to cook under certain conditions, and the pulp yield is 50%-54%. A low eutectic solvent is a clear and transparent homogeneous solvent formed by two or three components through hydrogen bond interactions between hydrogen bond donors and hydrogen bond acceptors. Low eutectic solvents have the advantages of being non-toxic, recyclable, and stable. Research on the clean pulping process of bamboo pulp with low eutectic solvents has important practical significance for the pulp and paper industry.
[0004] However, the existing pulping technology using bamboo as the main raw material has at least the following disadvantages:
[0005] Since cellulose, hemicellulose and lignin are closely combined in bamboo raw materials, existing pulping technology often uses more intense cooking conditions to achieve the purpose of removing a large amount of lignin, but at the same time, cellulose is partially degraded during the pulping process, reducing the pulp yield. Although the mild pulping technology currently developed has solved some of the problems existing in the existing technology, it still has many disadvantages, such as high environmental pollution load of traditional alkali liquid cooking, cumbersome processing process, low yield, high cost of reagents used in new low eutectic solvents, and reduced cellulose yield. Summary of the invention
[0006] In view of the above-mentioned shortcomings, the present invention provides a method for preparing pulp by steaming bamboo raw materials with a ternary low eutectic solvent. The method has the advantages of easy availability of reagents, environmental friendliness and high pulp yield.
[0007] The present invention provides a method for preparing pulp by steaming bamboo raw materials with a ternary deep eutectic solvent, which comprises the following steps:
[0008] S1: mixing the bamboo material and the ternary low eutectic solvent in proportion, and reacting them in a microwave at 120° C. to 140° C. and a power of 500 W to 700 W for 10 min to 30 min;
[0009] S2 is then washed with acetone solution, anhydrous ethanol, and deionized water in sequence until it becomes neutral, and then dried to obtain a fiber residue, that is, the target slurry;
[0010] The preparation method of the ternary low eutectic solvent is as follows: at a temperature of 70° C. to 90° C., choline chloride, amino acid and L-lactic acid solution are mixed in proportion, and heating and stirring are continued until a clear and transparent solution is formed to obtain a ternary low eutectic solvent.
[0011] In a specific implementation manner, the bamboo raw material is selected from moso bamboo, cycad bamboo, etc., which are crushed into 30-50 meshes to initially obtain the bamboo raw material.
[0012] In a preferred embodiment, the acetone solution in S2 is a 50% acetone solution.
[0013] In a specific embodiment, the amino acid is one or more of L-arginine, L-tyrosine, L-glycine, L-alanine, L-proline, L-valine, and L-threonine.
[0014] In a preferred embodiment, the mixing ratio of choline chloride, amino acid and L-lactic acid is 1:0.01-0.1:2-18, preferably 1:0.03-0.08:6-15, and more preferably 1:0.05:9.
[0015] In a specific implementation manner, the mixing ratio of the choline chloride, amino acid and L-lactic acid is 1:0.0-4-0.06:7-11; specifically 1:0.05:9.
[0016] Preferably, in S1, the reaction is carried out in a microwave apparatus at 125° C. to 135° C. and a power of 500 W to 700 W for 15 min to 25 min. More specifically, for example, the temperature is 130° C. and the microwave power is 600 W, and the reaction is carried out under these conditions for 20 min.
[0017] The present invention also provides the slurry obtained by the method.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] Compared with the prior art, the method for preparing pulp by treating bamboo with ternary low eutectic solvent-assisted microwaves in the present invention uses a low eutectic solvent to pretreat bamboo, thereby improving the pulp yield; the present invention uses a microwave reactor to assist in cooking under limited conditions, greatly shortening the cooking time and significantly improving the cooking efficiency. Since the power, cooking time and temperature of the microwave reactor are used in the research, the present invention achieves the goal of taking into account the cooking effect while preventing excessive damage to the internal structure of the raw material by microwaves.
[0020] In addition, the addition of amino acids can significantly increase the pulp retention rate and effectively improve the pulping effect of the low eutectic solvent. The principle is that amino acids can form an intermolecular hydrogen bond with one of the three hydroxyl groups on the same side of cellulose, thereby preventing the choline cations and protons, or chloride anions and carboxylic acid anions in the low eutectic solvent from simultaneously forming three hydrogen bonds with the three hydroxyl groups on the same side of cellulose, thereby inhibiting the degradation of cellulose.
[0021] Therefore, the clean pulping process using bamboo as pulping raw material provided by the present invention produces very little black liquor and no harmful gas during the process, and the generated waste and pulping waste liquid can be recycled and reused by evaporation and other methods. DETAILED DESCRIPTION
[0022] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0023] Unless otherwise specified, the test methods used in the embodiments of the present invention are all conventional methods.
[0024] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0025] Example 1
[0026] 1. Material preparation: crush the bamboo into 40 meshes to complete the material preparation;
[0027] 2. Synthesis of a low eutectic solvent: A low eutectic solvent was synthesized with a molar ratio of choline chloride, L-arginine, and L-lactic acid of 1:0.05:9. The three components were mixed in a flask, placed in an 80°C oil bath and stirred until a clear and transparent solution was formed;
[0028] 3. Pretreatment: Add 40-mesh bamboo powder into a flask containing a low eutectic solvent at a mass ratio of 1:20, place the flask in a microwave reactor, adjust the temperature to 130°C, the microwave power to 600W, and maintain this condition for 20 minutes. After the pretreatment, a mixed slurry is obtained;
[0029] 4. Washing: Use 50% acetone solution with 3 times the volume of the low eutectic solvent to wash the mixed slurry. The washing operation is performed using a vacuum filter. After the acetone washing is completed, continue to wash the slurry with anhydrous ethanol. After the washing liquid becomes colorless, continue washing with deionized water until the pH value of the washing liquid is neutral;
[0030] 5. Drying: Place the slurry obtained in step (4) in an oven and dry for 24 hours to obtain the target slurry.
[0031] Example 2
[0032] 1. Material preparation: crush the bamboo into 40 meshes to complete the material preparation;
[0033] 2. Synthesis of a low eutectic solvent: A low eutectic solvent was synthesized with a molar ratio of choline chloride, L-tyrosine, and L-lactic acid of 1:0.05:9. The three components were mixed in a flask, placed in an 80°C oil bath and stirred until a clear and transparent solution was formed;
[0034] 3. Pretreatment: Add 40-mesh bamboo powder into a flask containing a low eutectic solvent at a mass ratio of 1:20, place the flask in a microwave reactor, adjust the temperature to 130°C, the microwave power to 600W, and maintain this condition for 20 minutes. After the pretreatment, a mixed slurry is obtained;
[0035] 4. Washing: Use 50% acetone solution with 3 times the volume of the low eutectic solvent to wash the mixed slurry. The washing operation is performed using a vacuum filter. After the acetone washing is completed, continue to wash the slurry with anhydrous ethanol. After the washing liquid becomes colorless, continue washing with deionized water until the pH value of the washing liquid is neutral;
[0036] 5. Drying: Place the slurry obtained in step (4) in an oven and dry for 24 hours to obtain the target slurry.
[0037] Example 3
[0038] 1. Material preparation: crush the bamboo into 40 meshes to complete the material preparation;
[0039] 2. Synthesis of a low eutectic solvent: A low eutectic solvent was synthesized with a molar ratio of choline chloride, L-glycine, and L-lactic acid of 1:0.05:9. The three components were mixed in a flask, placed in an 80°C oil bath and stirred until a clear and transparent solution was formed;
[0040] 3. Pretreatment: Add 40-mesh bamboo powder into a flask containing a low eutectic solvent at a mass ratio of 1:20, place the flask in a microwave reactor, adjust the temperature to 130°C, the microwave power to 600W, and maintain this condition for 20 minutes. After the pretreatment, a mixed slurry is obtained;
[0041] 4. Washing: Use 50% acetone solution with 3 times the volume of the low eutectic solvent to wash the mixed slurry. The washing operation is performed using a vacuum filter. After the acetone washing is completed, continue to wash the slurry with anhydrous ethanol. After the washing liquid becomes colorless, continue washing with deionized water until the pH value of the washing liquid is neutral;
[0042] 5. Drying: Place the slurry obtained in step (4) in an oven and dry for 24 hours to obtain the target slurry.
[0043] Example 4
[0044] 1. Material preparation: crush the bamboo to 40 meshes to complete the material preparation;
[0045] 2. Synthesis of a low eutectic solvent: A low eutectic solvent was synthesized with a molar ratio of choline chloride, L-glycine, and L-lactic acid of 1:0.05:9. The three components were mixed in a flask, placed in an 80°C oil bath and stirred until a clear and transparent solution was formed;
[0046] 3. Pretreatment: Add 40-mesh bamboo powder into a flask containing a low eutectic solvent at a mass ratio of 1:20, place the flask in a microwave reactor, adjust the temperature to 130°C, the microwave power to 600W, and maintain this condition for 20 minutes. After the pretreatment, a mixed slurry is obtained;
[0047] 4. Washing: Use 50% acetone solution with 3 times the volume of the low eutectic solvent to wash the mixed slurry. The washing operation is performed using a vacuum filter. After the acetone washing is completed, continue to wash the slurry with anhydrous ethanol. After the washing liquid becomes colorless, continue washing with deionized water until the pH value of the washing liquid is neutral;
[0048] 5. Drying: Place the slurry obtained in step (4) in an oven and dry for 24 hours to obtain the target slurry.
[0049] Comparative Example 1
[0050] 1. Material preparation: crush the bamboo into 40 meshes to complete the material preparation;
[0051] 2. Synthesis of deep eutectic solvent: Synthesize a deep eutectic solvent with a molar ratio of choline chloride and L-lactic acid of 1:9. Mix the three components in a flask, place in an 80°C oil bath and stir until a clear and transparent solution is formed;
[0052] 3. The various operations and parameter settings during the pulping process refer to the above-mentioned Example 1.
[0053] The pulp yield results obtained in the above pulping process are shown in Table 1 below.
[0054] Table 1 Slurry yield results
[0055] project Slurry yield Example 1 64% Example 2 58% Example 3 59% Example 4 61% Comparative Example 1 48%
[0056] As can be seen from the above table, the present invention uses bamboo and bamboo as raw materials, and after microwave-assisted low eutectic solvent pretreatment, the pulp yield is about 60%, while the pulp yield of the comparative example is less than 50%. It can be seen that when adding amino acids as cellulose protective agents, the low eutectic solvent using choline chloride and L-lactic acid as hydrogen bond acceptors and hydrogen bond donors can effectively protect cellulose from degradation during cooking and improve the pulp yield.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing pulp by steaming bamboo raw materials with a ternary deep eutectic solvent, It is characterized in that The method comprises the following steps: S1: mixing the bamboo material and the ternary low eutectic solvent in proportion, and reacting them in a microwave at 120° C. to 140° C. and a power of 500 W to 700 W for 10 min to 30 min; S2 is then washed with acetone solution, anhydrous ethanol, and deionized water in sequence until it becomes neutral, and then dried to obtain a fiber residue, that is, the target slurry; The preparation method of the ternary low eutectic solvent is as follows: under the condition of a temperature of 70° C. to 90° C., choline chloride, amino acid and L-lactic acid solution are mixed in proportion, and heating and stirring are continued until a clear and transparent solution is formed to obtain a ternary low eutectic solvent.
2. The method according to claim 1, It is characterized in that The raw material is selected from moso bamboo, bamboo shoots and the like, and is crushed into 30-50 meshes to preliminarily obtain the raw material.
3. The method according to claim 1, It is characterized in that The acetone solution in S2 is a 50% acetone solution.
4. The method according to claim 1, It is characterized in that The amino acid is one or more of L-arginine, L-tyrosine, L-glycine, L-alanine, L-proline, L-valine and L-threonine.
5. The method according to claim 1, It is characterized in that The mixing ratio of the choline chloride, amino acid and L-lactic acid is 1: 0.01-0.1: 2-18.
6. The method according to claim 5, It is characterized in that The mixing ratio of the choline chloride, amino acid and L-lactic acid is 1: 0.03-0.08:6-15; more preferably 1: 0.05:
9.
7. The method according to claim 1, It is characterized in that The mixing ratio of the choline chloride, amino acid and L-lactic acid is 1: 0.0-4-0.06:7-11; specifically 1: 0.05:
9.
8. The method according to claim 1, It is characterized in that In S1, the reaction is carried out in a microwave apparatus at 125°C to 135°C and a power of 500W to 700W for 15min to 25min.
9. The method according to claim 1, It is characterized in that In S1, the reaction was carried out in a microwave apparatus at 130° C. and a microwave power of 600 W for 20 min.
10. The slurry obtained by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
A preparation method of bleached bamboo pulp
CN116145457B
Clean pulping process of bamboo and straw
CN116200959B
Sulfate bamboo pulp DDS cooking process
CN116695479A
Method for pretreating lignocellulose by adopting alkaline eutectic solvent
CN108441530A
Eutectic solvent and application of eutectic solvent in lignin extraction
CN110540508A