Reinforcing method and reinforcing structure for eccentric compression steel pipe concrete
By bonding FRP sheets along the axis direction in the steel pipe concrete tension zone and applying pressure using threaded parts and anchors, the problems of poor reinforcement effect and high cost of eccentric compressed steel pipe concrete are solved, and better reinforcement effect and cost are achieved Savings, while suppressing space-removing diseases, improving load-bearing capacity and service performance.
Patent Information
- Application Number
- CN202411318663.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-12
AI Technical Summary
In the reinforcement of eccentric compressed steel pipe concrete, the winding direction of the FRP sheet is perpendicular to the axial direction, resulting in a reduction in the reinforcement effect, and the cost is high, and the steel pipe concrete is prone to decay and decay, affecting the load-bearing capacity and service performance.
The FRP sheet is bonded in the tension zone of the steel pipe concrete along the axis direction, and pressure is applied through the threaded parts and anchors. The FRP sheet is distributed along the axis direction. The threaded parts pass through the internal concrete of the steel pipe concrete to prevent de-emphasis and save FRP sheet Dosage and construction cost.
It improves the reinforcement effect of eccentric compressed steel pipe concrete, reduces construction costs, inhibits the separation between the concrete and the inner wall of the steel pipe, and enhances the load-bearing capacity and service performance.
Smart Images

Figure CN118933398A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel tube concrete reinforcement, and in particular to an eccentrically compressed steel tube concrete reinforcement method and a reinforcement structure. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] As an effective composite structure, steel tube concrete has always been valued by the civil engineering community for its superior performance. In addition to its mechanical properties such as high strength, light weight, good ductility, fatigue resistance, and impact resistance, it also has excellent construction performance such as saving labor and materials, easy erection, and fast construction. It is widely used in single-story and multi-story industrial plant columns, various brackets, truss struts, piles, high-rise and super-high-rise buildings, arch bridges, and composite beam bridge structures. With the continuous deepening of the application and research of steel tube concrete structures, researchers have found that the core concrete in steel tube concrete has plastic shrinkage, autogenous shrinkage, creep shrinkage and other problems, which cause the core concrete in steel tube concrete to be emptied and debonded from the steel tube wall. The above phenomenon will also occur under the influence of ambient temperature and light, reducing the service performance and bearing capacity of steel tube concrete. In addition, the load types to which steel tube concrete is subjected in different engineering structures are also different. Due to the low tensile strength of concrete, when subjected to high eccentric loads, cracks are very likely to occur on the outside of the core concrete on the tensile side of steel tube concrete. If not treated, bending damage of steel tube concrete is very likely to occur, affecting the service performance of the structure and thus affecting people's traffic safety.
[0004] For the reinforcement and repair of steel tube concrete, scholars have proposed a method of using FRP sheets to wrap around the outside of the steel tube for reinforcement. This method effectively improves the insufficient bearing capacity of steel tube concrete. However, for eccentrically compressed steel tube concrete components, the direction of the FRP sheet wrapping the steel tube is perpendicular to the axial direction, which greatly reduces the reinforcement effect of this method on the eccentrically compressed components. In addition, this method uses a large amount of FRP sheets, and the reinforcement cost is relatively high. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an eccentrically compressed steel tube concrete reinforcement method and reinforcement structure, which has good reinforcement effect on eccentrically compressed steel tube concrete and low reinforcement cost, and can inhibit the occurrence of concrete voiding defects inside the steel tube concrete, thereby improving the bearing capacity and service performance of the steel tube concrete.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, an embodiment of the present invention provides a method for reinforcing an eccentrically compressed concrete-filled steel tube, comprising the following steps:
[0008] At least one set of FRP sheets is bonded to the tensile zone of the steel tube concrete, and the FRP sheets are arranged along the axial direction of the steel tube concrete;
[0009] A plurality of threaded members are constructed on both sides of the FRP sheet, and the threaded members pass through the steel tube of the steel tube concrete and are implanted into the concrete inside the steel tube concrete;
[0010] Anchors are installed, the anchors are pressed against the outer surface of the FRP sheet, the threaded piece passes through the anchors and is threadedly connected to the locking piece, and the locking piece is rotated so that the anchors apply a set pressure load to the FRP sheet.
[0011] Optionally, when multiple groups of FRP sheets are bonded to the tensile zone of the steel tube concrete, the multiple groups of FRP sheets are distributed circumferentially along the steel tube concrete, and multiple anchors on the outer sides of adjacent FRP sheets are staggered.
[0012] Optionally, the same group of FRP sheets includes at least one FRP sheet. When the same group has multiple FRP sheets, the multiple FRP sheets are stacked and bonded in sequence.
[0013] Optionally, the FRP sheet is impregnated with epoxy resin and then bonded and fixed to the tensile zone of the steel tube concrete.
[0014] Optionally, before bonding the FRP sheets, the FRP sheet bonding area in the tensile zone of the steel tube concrete is polished and rust-removed.
[0015] Optionally, the distance between the threaded member and the edge of the FRP sheet on the same side is not greater than 2 cm.
[0016] Optionally, the construction method of the threaded member comprises the following steps:
[0017] A through hole is drilled in the steel tube of the steel tube concrete-filled structure, wherein the through hole extends to the outer side surface of the concrete inside the steel tube concrete-filled structure;
[0018] Then a channel coaxial with the through hole is punched in the concrete;
[0019] After the threaded part passes through the through hole, it is implanted into the channel through the anchor glue and cured until the strength of the anchor glue reaches the set strength.
[0020] Optionally, the diameter of the through hole is larger than the channel diameter by 3.5 mm to 4.5 mm, preferably by 4 mm.
[0021] Optionally, a rubber cushion layer is inserted between the anchor and the outer surface of the steel tube concrete before tightening the locking piece.
[0022] In the second aspect, an embodiment of the present invention provides an eccentrically compressed steel tube concrete reinforcement structure, which is reinforced by the eccentrically compressed steel tube concrete reinforcement method described in the first aspect, and includes at least one group of FRP sheets bonded and fixed to the tensile zone of the steel tube concrete, the FRP sheets are arranged along the axial direction of the steel tube concrete, and multiple threaded parts are arranged on both sides of the FRP sheets. The threaded parts pass through the steel tube concrete steel pipe and are inserted into the internal concrete. Anchors are pressed on the outer side of the FRP sheets, the anchors pass through the threaded parts, the threaded parts are threadedly connected to the locking parts, and the locking parts are pressed on the outer surface of the anchors so that the anchors apply a set pressure load to the FRP sheets.
[0023] The beneficial effects of the present invention are as follows:
[0024] 1. In the reinforcement method and reinforcement structure of the present invention, the FRP sheets are distributed along the axis direction of the steel tube concrete. Compared with the traditional distribution method perpendicular to the axis of the steel tube concrete, the reinforcement effect for the eccentrically compressed steel tube concrete is better, and the problem of the lack of reinforcement method for the tensile zone of the eccentrically compressed steel tube concrete is solved. Moreover, the FRP sheets are only bonded in the set area of the tensile zone. Compared with the method of winding the FRP sheets, the FRP sheets do not need to cover the entire surface of the tensile zone, which saves the amount of FRP sheets and saves construction costs.
[0025] 2. In the reinforcement method and reinforcement structure of the present invention, the anchors press the FRP sheets against the outer surface of the steel tube concrete, further improving the reinforcement effect of the FRP sheets on the steel tube concrete.
[0026] 3. In the reinforcement method and reinforcement structure of the present invention, the threaded parts are implanted into the concrete inside the steel tube concrete after passing through the steel tube of the steel tube concrete. The threaded parts inside the steel tube concrete exert a reaction force on the concrete, inhibiting the separation of the concrete from the inner wall of the steel tube, thereby achieving the technical effect of inhibiting the occurrence of void damage and improving the bearing capacity and service performance of the steel tube concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 is a flow chart of the reinforcement method of embodiment 1 of the present invention;
[0029] Figure 2 is a schematic diagram of the reinforcement structure of Example 2 of the present invention;
[0030] Figure 3 is a top view of the reinforcement structure of Example 2 of the present invention;
[0031] Figure 4This is a schematic diagram of the coordination of the anchor, threaded member, locking member and rubber cushion layer in Embodiment 2 of the present invention;
[0032] Figure 5 2 is a schematic diagram of the distribution of anchors and screws when multiple groups of FRP sheets are provided in Example 2 of the present invention;
[0033] Among them, 1. Concrete, 2. Steel pipe, 3. Stud, 4. Anchor, 5. FRP sheet, 6. Rubber cushion, 7. Washer, 8. Nut. DETAILED DESCRIPTION
[0034] Example 1
[0035] This embodiment provides an eccentrically compressed steel tube concrete reinforcement method, wherein the steel tube concrete comprises an outer steel tube 2, and the steel tube has a core concrete 1 inside, and the core concrete is cast inside the steel tube, such as Figure 1 As shown, the following steps are included:
[0036] Step 1: Determine the pasting position of the FRP sheet 5 in the tensile area of the steel tube concrete, define the pasting position as the calibration position, and grind and remove rust from the calibration position using sandpaper or grinding equipment to ensure that there are no other impurities that affect the interface bonding properties on the contact surface between the FRP sheet 5 and the steel tube of the steel tube concrete.
[0037] Step 2: After cleaning, start pasting the FRP sheet 5. In this embodiment, there is at least one calibrated position, so at least one corresponding FRP sheet 5 is set. Each group of FRP sheets 5 corresponds to a calibrated position. The same group of FRP sheets 5 includes at least one stacked sheet. The length direction of the FRP sheet 5 is set along the axial direction of the steel tube concrete.
[0038] When pasting, first soak the FRP sheet 5 with epoxy resin glue, and then paste the FRP sheet 5 on the marked position of the outer surface of the steel pipe 2. If the same group of FRP sheets 5 includes multiple sheets stacked, the FRP sheets 5 are stacked and bonded in sequence.
[0039] Step 3: After the FRP sheet 5 is pasted and cured, the positions of the screw parts are located on both sides of the FRP sheet 5. In this embodiment, the screw parts are studs 3, and the distance between the position of the studs 3 and the edge of the same side of the FRP sheet 5 is less than 2 cm to ensure that the anchor 4 applies pressure to the FRP sheet 5.
[0040] When a plurality of groups of FRP sheets 5 are arranged in the tension zone, the positions of the studs 3 of adjacent FRP sheets are staggered, that is, the subsequent anchors 4 are staggered to prevent the occurrence of stress concentration caused by the studs 3 .
[0041] Step 4: After the stud 3 is positioned, the construction of the stud 3 begins. A metal hole opener is used to punch a hole in the steel pipe 2. The formed through hole extends to the surface of the concrete 1. That is, the metal hole opener stops when it touches the surface of the concrete 1. Then, the process of punching the concrete 1 begins to form a channel opened in the concrete 1 and coaxial with the through hole.
[0042] In this embodiment, the diameter of the through hole is larger than the diameter of the channel by 3.5mm-4.5mm, preferably 4mm. After the channel is completed, the stud 3 is passed through the through hole and implanted into the channel using anchor glue, and then cured until the strength of the anchor glue reaches the set strength.
[0043] Step 5: Install anchors 4 at the studs 3 corresponding to the two sides of the FRP sheet 5. The anchors 4 are arc-shaped anchor plates that match the steel pipes 2. Openings for the studs 3 to pass through are provided on both sides of the anchor plates. The anchor plates are arranged on the outside of the FRP sheet 5. The studs 3 pass through the anchor plates through the openings. The part of the studs 3 that passes through the anchor plates is threadedly connected with a locking piece. The locking piece can be a nut 8. A washer 7 is inserted between the nut 8 and the anchor plate.
[0044] Step 6: insert a rubber pad 6 between the anchor plate and the FRP sheet 5, the rubber pad 6 fits with the outer surface of the FRP sheet 5 to ensure that the pressure applied by the anchor 4 is transmitted to the FRP sheet 5, use a torque wrench to apply torque to the nut 8 to drive 8 to rotate, the nut 8 applies pressure to the anchor plate through the washer 7, and the anchor plate applies pressure to the FRP sheet 5 through the rubber pad 6 until the pressure applied by the nuts 8 on both sides of the anchor plate increases to the same set pressure value. The group finally completes the reinforcement of the eccentrically compressed steel tube concrete, and the anchor 4 presses the FRP sheet 5 against the outer surface of the steel tube concrete, further improving the reinforcement effect of the FRP sheet on the steel tube concrete.
[0045] The reinforcement method of this embodiment is convenient and fast in construction, saving time and labor costs. The FRP sheet 5 is distributed along the axial direction of the steel tube concrete. Compared with the traditional distribution method perpendicular to the axis of the steel tube concrete, it has a better reinforcement effect on the eccentrically compressed steel tube concrete, and solves the problem of the lack of reinforcement method for the tensile zone of the eccentrically compressed steel tube concrete. Moreover, the FRP sheet 5 is only bonded in the set area of the tensile zone. Compared with the method of winding the FRP sheet, the FRP sheet does not need to cover the entire tensile zone surface, which saves the amount of FRP sheet and the construction cost. Moreover, the stud 3 passes through the steel tube of the steel tube concrete and is implanted into the concrete inside it. The stud inside the steel tube concrete exerts a reaction force on the concrete, inhibiting the separation of the concrete and the inner wall of the steel tube, thereby achieving the technical effect of inhibiting the occurrence of void damage and improving the bearing capacity and service performance of the steel tube concrete.
[0046] Example 2
[0047] This embodiment provides an eccentrically compressed steel tube concrete reinforcement structure, which is constructed using the eccentrically compressed steel tube concrete reinforcement method described in Example 1. Figure 2-Figure 4 As shown, it includes steel tube concrete, which includes a steel tube 2, and concrete 1 is arranged inside. The tensile zone of the steel tube concrete is provided with at least one calibration position for reinforcement, and the calibration position is bonded with an FRP sheet 5 by epoxy resin glue. The FRP sheet 5 is arranged along the axial direction of the steel tube concrete. A plurality of threaded members are arranged on both sides of the FRP sheet 5. The threaded member adopts a stud 3. The distance between the stud 3 and the same side edge of the FRP sheet 5 is not greater than 2 cm. The stud 3 passes through the steel tube 2 and is placed in the concrete 1 An anchor 4 is provided between the two corresponding studs 3 on both sides of the FRP sheet 5. The anchor 4 adopts an anchor plate. The corresponding stud 3 passes through the anchor plate through the openings provided at both ends of the anchor plate and is threadedly connected with a locking piece. The locking piece adopts a nut 8. A rubber pad 6 is provided between the anchor plate and the FRP sheet 5. A washer 7 is provided between the nut 8 and the anchor plate and is sleeved on the outer periphery of the stud 3. The nut 8 is tightened and pressed against the outer surface of the anchor plate. The anchor plate applies a set pressure load to the FRP sheet 5 through the rubber pad 6.
[0048] One or more groups of FRP sheets 5 are arranged in the tension zone of the steel tube concrete, such as Figure 5 As shown, when multiple groups of FRP sheets 5 are bonded, the anchor plates of adjacent FRP sheets 5 are staggered to prevent stress concentration caused by the studs 3, and the same group of FRP sheets 5 is formed by one or more stacked and bonded sheets.
[0049] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for reinforcing eccentrically compressed concrete-filled steel tubes, characterized in that: The following steps are involved: At least one set of FRP sheets is bonded to the tensile zone of the steel tube concrete, and the FRP sheets are arranged along the axial direction of the steel tube concrete; A plurality of threaded members are constructed on both sides of the FRP sheet, and the threaded members pass through the steel tube of the steel tube concrete and are implanted into the concrete inside the steel tube concrete; Anchors are installed, the anchors are pressed against the outer surface of the FRP sheet, the threaded piece passes through the anchors and is threadedly connected to the locking piece, and the locking piece is rotated so that the anchors apply a set pressure load to the FRP sheet.
2. The eccentrically compressed steel tube concrete reinforcement method according to claim 1, characterized in that: When multiple groups of FRP sheets are bonded to the tensile zone of the steel tube concrete, the multiple groups of FRP sheets are distributed along the circumferential direction of the steel tube concrete, and multiple anchors on the outer sides of adjacent FRP sheets are staggered.
3. The eccentrically compressed concrete-filled steel tube reinforcement method according to claim 1, characterized in that: The same group of FRP sheets includes at least one FRP sheet. When the same group includes multiple FRP sheets, the multiple FRP sheets are stacked and bonded in sequence.
4. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 1, characterized in that: After the FRP sheet is impregnated with epoxy resin, it is bonded and fixed to the tensile zone of the steel tube concrete.
5. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 1, characterized in that: Before bonding the FRP sheets, the FRP sheet bonding area in the tensile zone of the steel tube concrete is polished and rust-removed.
6. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 1, characterized in that: The distance between the threaded member and the edge of the FRP sheet on the same side is not greater than 2 cm.
7. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 1, characterized in that: The construction method of the threaded member comprises the following steps: A through hole is drilled in the steel tube of the steel tube concrete-filled structure, wherein the through hole extends to the outer side surface of the concrete inside the steel tube concrete-filled structure; Then a channel coaxial with the through hole is punched in the concrete; After the threaded part passes through the through hole, it is implanted into the channel through the anchor glue and cured until the strength of the anchor glue reaches the set strength.
8. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 7, characterized in that: The diameter of the through hole is 3.5 mm to 4.5 mm larger than the channel diameter, preferably 4 mm.
9. The method for reinforcing eccentrically compressed concrete-filled steel tubes according to claim 1, characterized in that: After inserting a rubber cushion between the anchor and the outer surface of the steel tube concrete, the locking piece is tightened.
10. An eccentrically compressed steel tube concrete reinforced structure, characterized in that: The eccentrically compressed steel tube concrete reinforcement method according to any one of claims 1 to 9 is used for reinforcement, and comprises at least one group of FRP sheets bonded and fixed in the tensile zone of the steel tube concrete, the FRP sheets are arranged along the axial direction of the steel tube concrete, a plurality of threaded members are arranged on both sides of the FRP sheets, the threaded members pass through the steel tube concrete tube and are inserted into the internal concrete, an anchor is pressed on the outer side of the FRP sheet, the anchor passes through the threaded member, the threaded member is threadedly connected to a locking member, and the locking member is pressed on the outer surface of the anchor so that the anchor applies a set pressure load to the FRP sheet.
Citation Information
Patent Citations
Steel tube concrete column and manufacturing method thereof
CN108277925A
Method for calculating large eccentric bearing capacity of high-strength steel bar steel fiber concrete short column
CN118364557A
Fiber cloth anchor device for reinforcing externally bonded fiber cloth in concrete structure
CN201439646U
Unilateral package steel reinforced concrete column
CN206737464U
Take off hollow steel tube concrete strengthening structure
CN207863514U