Porous molybdenum composite heat pipe and preparation method thereof
By adopting porous molybdenum composite heat pipe structure in ultra-high temperature heat pipes, and using porous molybdenum liquid absorbing cores with molybdenum tube shells, ultra-fine porous molybdenum layer and multi-step trench structures, the insufficient preparation and heat transfer performance of ultra-high temperature heat pipes in the existing technology is solved. The problem of this has achieved efficient heat transfer performance improvement.
Patent Information
- Application Number
- CN202411301988.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-18
AI Technical Summary
It is difficult to prepare ultra-high temperature heat pipes with working temperatures above 1300K, and the structure of the metal porous liquid absorbing core has little impact on the heat transfer performance of the heat pipe.
The porous molybdenum composite heat pipe is adopted, consisting of a molybdenum tube shell, an ultra-fine porous molybdenum layer and a porous molybdenum liquid absorbing core with a multi-step trench structure. It is formed by sintering and cold isostatic pressing technology to increase capillary pressure to enhance heat transfer performance.
The preparation of porous molybdenum composite heat pipe with a working temperature of more than 1300K is achieved, which significantly improves the heat transfer performance and structural strength of the heat pipe, and is suitable for higher temperature applications.
Smart Images

Figure CN118936174A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal porous liquid wick and metal porous material preparation, and specifically relates to a porous molybdenum composite heat pipe and a preparation method thereof. Background Art
[0002] When the heat pipe is working, it uses the gasification of the working fluid to absorb heat, and then liquefies at the cold source to release heat. At the same time, the capillary force provided by the porous wick of the heat pipe drives the working fluid back to the evaporation section of the heat pipe, thereby ensuring that the working fluid absorbs heat again and gasifies to achieve cyclic heat dissipation. As an important component of the heat pipe, the metal porous wick not only provides a channel for the flow of the working fluid, but also generates capillary force to drive the working fluid back to the evaporation section. Therefore, the structure of the metal porous wick directly affects the heat transfer performance of the heat pipe.
[0003] Heat pipes can be divided into low-temperature heat pipes, normal-temperature heat pipes, medium-temperature heat pipes, high-temperature heat pipes and ultra-high-temperature heat pipes according to their working temperature. At present, the working temperature of most heat pipes used in scientific research and production is below 1300K, and its theoretical and applied research has been increasingly improved, while the preparation research of ultra-high-temperature heat pipes with working temperature above 1300K needs to be further strengthened.
[0004] Therefore, a porous molybdenum composite heat pipe with an operating temperature above 1300K and a preparation method thereof are needed. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a porous molybdenum composite heat pipe in view of the deficiencies of the above-mentioned prior art. The porous molybdenum composite heat pipe provides structural strength by setting a molybdenum tube shell as the base layer of the porous molybdenum composite heat pipe, plays a supporting and sealing role, and effectively promotes the sintering and bonding of the molybdenum tube and the porous molybdenum wick by setting an ultrafine porous molybdenum layer. By setting a porous molybdenum wick and introducing a multi-step groove structure, a larger capillary pressure is provided for the porous molybdenum wick, thereby enhancing the heat transfer performance of the porous molybdenum composite heat pipe, making it suitable for higher operating temperatures, and obtaining a porous molybdenum composite heat pipe with an operating temperature above 1300K.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a porous molybdenum composite heat pipe, characterized in that the porous molybdenum composite heat pipe is composed of a molybdenum tube shell, an ultrafine porous molybdenum layer and a porous molybdenum liquid absorption core with a multi-step groove structure from the outside to the inside.
[0007] The above-mentioned porous molybdenum composite heat pipe is characterized in that the wall thickness of the molybdenum tube shell is 1mm~2mm, the thickness of the ultrafine porous molybdenum layer is 0.5mm~0.8mm, the pore size of the porous structure in the ultrafine porous molybdenum layer is 0.5μm~1.5μm, the thickness of the porous molybdenum liquid absorption core is 3.6mm~3.8mm, the pore size of the porous structure in the porous molybdenum liquid absorption core is 5μm~25μm, and the depth of the multi-step groove structure is 0.8mm~3.4mm.
[0008] The above-mentioned porous molybdenum composite heat pipe is characterized in that the multi-step groove structure is divided into multiple groups, each group of the multi-step groove structure includes 3 to 9 grooves, and the groove depth first gradually increases and then decreases step by step.
[0009] In addition, the present invention also provides a method for preparing a porous molybdenum composite heat pipe, characterized in that the method comprises the following steps:
[0010] Step 1: Grind the inner wall of the molybdenum tube, and then process the threads to obtain a threaded molybdenum tube shell;
[0011] Step 2: dispersing molybdenum powder into an ethanol solution of polyvinyl butyral and stirring the mixture to obtain a molybdenum powder slurry;
[0012] Step 3: coating the inner wall of the threaded molybdenum tube shell obtained in step 1 with the molybdenum powder slurry obtained in step 2, and then sintering the inner wall under a hydrogen atmosphere to obtain a molybdenum tube shell having an ultrafine porous molybdenum layer;
[0013] Step 4: The molybdenum tube shell with the ultrafine porous molybdenum layer obtained in step 3 is used as a tube shell, and then filled with mixed molybdenum powder, and then cold isostatically pressed to obtain a cold isostatically pressed molybdenum tube shell;
[0014] Step 5, sintering the cold isostatically pressed molybdenum tube shell obtained in step 4 under a hydrogen atmosphere to obtain a sintered molybdenum tube shell;
[0015] Step 6: Process the inner wall of the sintered molybdenum tube shell obtained in step 5 into a multi-step groove structure to obtain a porous molybdenum composite heat pipe.
[0016] The above method is characterized in that the depth of the thread in step 1 is 0.3 mm to 0.5 mm. The present invention controls the depth of the thread so that the ultrafine porous molybdenum layer and the molybdenum tube have an excellent cross-linking depth, ensuring that the ultrafine porous molybdenum layer and the molybdenum tube are easy to form a metallurgical bond, and also enables the threaded molybdenum tube shell to have an optimal slurry hanging ability, so that the molybdenum powder slurry is excellently combined with the molybdenum tube, and it is convenient to prepare a molybdenum tube with an ultrafine porous molybdenum layer.
[0017] The above method is characterized in that the particle size of the molybdenum powder in step 2 is 0.5 μm to 2.5 μm, the mass fraction of polyvinyl butyral in the ethanol solution of polyvinyl butyral is 3% to 5%, and the concentration of molybdenum powder in the molybdenum powder slurry is 0.25 g / mL to 0.35 g / mL. The present invention controls the particle size of the molybdenum powder so that the porous structure in the ultrafine porous molybdenum layer has an excellent pore size, controls the amount of polyvinyl butyral so that the molybdenum powder slurry is hung on the inner wall of the threaded molybdenum tube shell, and controls the concentration of the molybdenum powder in the molybdenum powder slurry to control the quality of the ultrafine porous molybdenum layer, thereby ensuring the performance of the porous molybdenum composite heat pipe.
[0018] The above method is characterized in that the coating in step 3 is carried out by centrifugal coating, the coating thickness is 0.5 mm to 0.8 mm, the sintering temperature is 1200° C. to 1260° C., the time is 2 h, and the flow rate of hydrogen is 0.25 m 3 / h~0.4m 3 / h. The present invention controls the sintering parameters to fully sinter the molybdenum powder slurry to form an ultrafine porous molybdenum layer, and hydrogen, as a reducing agent with high ability to react with metal molybdenum, can reduce the molybdenum oxide on the surface of the molybdenum powder to metal molybdenum, which can not only improve the sintering activity of the molybdenum powder, but also promote the mutual diffusion between the metal molybdenum powders, thereby effectively improving the sintering strength of the porous molybdenum.
[0019] The above method is characterized in that the mixed molybdenum powder in step 4 is mixed with molybdenum powder with a particle size of 0.5μm to 2.5μm and molybdenum powder with a particle size of 15μm to 50μm in a mass ratio of 1 to 3:1, the cold isostatic pressing pressure is 160MPa to 200MPa, and the holding time is 30s to 150s. The present invention controls the particle size and ratio of the mixed molybdenum powder, mixes 0.5μm to 2.5μm molybdenum powder into 15μm to 50μm molybdenum powder, can effectively improve the sintering activity of molybdenum powder and realize the regulation of the porosity of porous molybdenum wick, and promotes the metallurgical bonding of porous molybdenum wick and a matrix with ultrafine molybdenum powder layer, and preforms the mixed molybdenum powder by controlling the parameters of cold isostatic pressing, which is convenient for subsequent sintering and ensures the performance of porous molybdenum composite heat pipe.
[0020] The above method is characterized in that the sintering temperature in step 5 is 1300°C to 1500°C, and the flow rate of hydrogen is 0.25m 3 / h~0.4m 3 / h. The present invention controls the sintering parameters to fully sinter the mixed molybdenum powder after cold isostatic pressing and stably connect it with the ultrafine porous molybdenum layer. In addition, hydrogen, as a reducing agent with high ability to react with metal molybdenum, can reduce the oxidized molybdenum on the surface of the molybdenum powder to metal molybdenum, which can not only improve the sintering activity of the molybdenum powder, but also promote the mutual diffusion between the metal molybdenum powders, thereby effectively improving the sintering strength of the porous molybdenum.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] 1. The present invention provides structural strength and plays a supporting and sealing role by arranging a molybdenum tube shell as the base layer of the porous molybdenum composite heat pipe. The ultrafine porous molybdenum layer is arranged to effectively promote the sintering and bonding of the molybdenum tube and the porous molybdenum wick. The porous molybdenum wick is arranged and a multi-step groove structure is introduced to provide a larger capillary pressure for the porous molybdenum wick, thereby enhancing the heat transfer performance of the porous molybdenum composite heat pipe, making it suitable for higher operating temperatures, and obtaining a porous molybdenum composite heat pipe with an operating temperature above 1300K.
[0023] 2. The present invention ensures the structural strength of the porous molybdenum composite heat pipe by controlling the wall thickness of the molybdenum tube shell, and has good sintering activity by controlling the thickness of the ultrafine porous molybdenum layer and the pore size of the porous structure. As an intermediate layer, it is helpful for the metallurgical bonding of the molybdenum tube shell and the porous molybdenum wick. By controlling the thickness, pore size and depth of the groove structure of the porous molybdenum wick, the capillary pressure of the porous molybdenum wick is increased, thereby enhancing the heat transfer performance of the composite molybdenum heat pipe.
[0024] 3. The present invention further optimizes the capillary pressure of the porous molybdenum wick and enhances the heat transfer performance of the composite molybdenum heat pipe by controlling the number of grooves in each group of the multi-step groove structure, and controls the groove depth to gradually increase and then decrease step by step, thereby increasing the specific surface area of the boiling working fluid at the evaporation end and enhancing the heat transfer capacity of the porous molybdenum micro heat pipe.
[0025] 4. The present invention controls the sintering parameters to fully sinter the molybdenum powder slurry to form an ultrafine porous molybdenum layer. Hydrogen, as a reducing agent with a high ability to react with metallic molybdenum, can reduce the molybdenum oxide on the surface of the molybdenum powder to metallic molybdenum, which can not only improve the sintering activity of the molybdenum powder, but also promote the mutual diffusion between metallic molybdenum powders, thereby effectively improving the sintering strength of the porous molybdenum.
[0026] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a schematic diagram of the structure of the multi-step groove structure porous molybdenum composite heat pipe of the present invention
[0028] Description of reference numerals:
[0029] 1—molybdenum tube shell; 2—ultrafine porous molybdenum layer; 3—porous molybdenum liquid wick;
[0030] 4—Multi-step groove structure. DETAILED DESCRIPTION
[0031] A porous molybdenum composite heat pipe of the present invention is described in detail through Example 1.
[0032] Example 1
[0033] like Figure 1 As shown, a porous molybdenum composite heat pipe of this embodiment is composed of a molybdenum tube shell 1, an ultrafine porous molybdenum layer 2 and a porous molybdenum liquid absorption core 3 with a multi-step groove structure 4 from the outside to the inside.
[0034] It should be noted that by setting the molybdenum tube shell 1 as the base layer of the porous molybdenum composite heat pipe, structural strength is provided to play a supporting and sealing role. By setting the ultrafine porous molybdenum layer 2, the sintering bonding of the molybdenum tube and the porous molybdenum wick 3 is effectively promoted. By setting the porous molybdenum wick 3 and introducing the multi-step groove structure 4, a larger capillary pressure is provided for the porous molybdenum wick 3, thereby enhancing the heat transfer performance of the porous molybdenum composite heat pipe, making it suitable for higher operating temperatures, and obtaining a porous molybdenum composite heat pipe with an operating temperature above 1300K.
[0035] In this embodiment, the wall thickness of the molybdenum tube shell 1 is 1mm-2mm, the thickness of the ultrafine porous molybdenum layer 2 is 0.5mm-0.8mm, the pore size of the porous structure in the ultrafine porous molybdenum layer 2 is 0.5μm-1.5μm, the thickness of the porous molybdenum wick 3 is 3.6mm-3.8mm, the pore size of the porous structure in the porous molybdenum wick 3 is 5μm-25μm, and the depth of the multi-step groove structure is 0.8mm-3.4mm. The structural strength of the porous molybdenum composite heat pipe is ensured by controlling the wall thickness of the molybdenum tube shell 1, and the thickness of the ultrafine porous molybdenum layer 2 and the pore size of the porous structure are controlled. The sintering activity is good, and as an intermediate layer, it is helpful for the metallurgical bonding of the molybdenum tube shell 1 and the porous molybdenum wick 3. The capillary pressure of the porous molybdenum wick 3 is increased by controlling the thickness, pore size and depth of the groove structure of the porous molybdenum wick 3, and the heat transfer performance of the composite molybdenum heat pipe is enhanced.
[0036] The above-mentioned porous molybdenum composite heat pipe is characterized in that the multi-step groove structure 4 is divided into multiple groups, each group of the multi-step groove structure 4 includes 3 to 9 grooves, and the groove depth first gradually increases and then decreases step by step. By controlling the number of grooves in each group of the multi-step groove structure 4, the capillary pressure of the porous molybdenum wick 3 is further optimized, the heat transfer performance of the composite molybdenum heat pipe is enhanced, and the groove depth is controlled to first gradually increase and then gradually decrease, thereby increasing the specific surface area of the boiling working medium at the evaporation end and enhancing the heat transfer capacity of the porous molybdenum micro heat pipe.
[0037] It should be noted that the theoretical calculation of the capillary pressure of the porous molybdenum composite heat pipe satisfies: ΔP=2σcosθ / r, where: ΔP is the capillary pressure of the porous molybdenum liquid wick 3, σ is the surface tension coefficient of the liquid, θ is the solid-liquid contact angle, and r is the effective capillary radius of the porous molybdenum liquid wick 3.
[0038] like Figure 1 As shown, when each group of multi-step groove structures 4 includes 7 grooves, and the groove depth first gradually increases and then gradually decreases, the capillary pressure of the porous liquid wick of the multi-step groove structure 4 can be divided into multiple parts, from left to right: the capillary pressure of the first-level step groove A, the capillary pressure of the second-level step groove B, the capillary pressure of the third-level step groove C, the capillary pressure of the fourth-level step groove D, the capillary pressure of the third-level step groove C, the capillary pressure of the second-level step groove B, the capillary pressure of the first-level step groove A, ..., the mathematical expression of the capillary pressure of the porous molybdenum composite heat pipe is: ΔP = n × 2σcosθ A / r Ac +2σcosθ B / r Bc +2σcosθ C / r Cc +2σcosθ D / r Dc +2σcosθ C / r Cc +2σcosθ B / r Bc +2σcosθ A / r Ac It can be seen from the above formula that the porous molybdenum wick 3 with a multi-step groove structure 4 can provide a larger capillary pressure than the ordinary directly pressed and sintered porous wick, so that the heat pipe has excellent heat transfer performance.
[0039] The preparation method of a porous molybdenum composite heat pipe of the present invention is described in detail through Examples 2 to 4.
[0040] Example 2
[0041] This embodiment includes the following steps:
[0042] Step 1: The inner wall of a molybdenum tube with a length of 100 mm, a wall thickness of 1 mm, and an outer diameter of 33 mm is polished with 280# and 180# sandpapers in turn, and then a thread with a depth of 0.5 mm is processed with a turning tool to obtain a threaded molybdenum tube shell;
[0043] Step 2: Disperse molybdenum powder with a particle size of 0.5 μm to 2.5 μm into an ethanol solution of 5% polyvinyl butyral by mass and stir well to obtain a molybdenum powder slurry;
[0044] Step 3: Use centrifugal coating to coat the inner wall of the threaded molybdenum tube shell obtained in step 1 with the molybdenum powder slurry obtained in step 2 with a thickness of 0.5 mm, and then 3 / h atmosphere to 1200°C and then sintered for 2h to obtain a molybdenum tube shell having an ultrafine porous molybdenum layer, wherein the maximum pore size of the ultrafine porous molybdenum layer is 1.5μm;
[0045] Step 4: The molybdenum tube shell with the ultrafine porous molybdenum layer obtained in step 3 is used as a tube shell, and then filled with mixed molybdenum powder formed by mixing molybdenum powder with a particle size of 0.5 μm to 2.5 μm and molybdenum powder with a particle size of 15 μm to 50 μm in a mass ratio of 1:1, and then placed in a cold isostatic pressing device for cold isostatic pressing at a pressure of 180 MPa and maintained for 150 seconds to obtain a cold isostatically pressed molybdenum tube shell;
[0046] Step 5: Place the cold isostatically pressed molybdenum shell obtained in step 4 under a hydrogen flow rate of 0.25 m 3 / h atmosphere to 1500°C for sintering to obtain a sintered molybdenum tube shell;
[0047] Step six, the inner wall of the sintered molybdenum tube shell obtained in step five is processed with a multi-step groove structure, each group of multi-step groove structures 4 includes 3 grooves, and the groove depth first gradually increases and then gradually decreases, to obtain a porous molybdenum composite heat pipe, the thickness of the ultrafine porous molybdenum layer 2 of the porous molybdenum composite heat pipe is 0.5mm, the maximum pore size is 0.5μm, the thickness of the porous molybdenum liquid wick 3 is 3.8mm, the maximum pore size is 25μm, and the depth of the groove structure is 0.8mm~3.4mm.
[0048] After testing, it was found that the porous molybdenum composite heat pipe prepared in this embodiment was used normally at a working temperature of 1300K.
[0049] Example 3
[0050] This embodiment includes the following steps:
[0051] Step 1: The inner wall of a molybdenum tube with a length of 100 mm, a wall thickness of 2 mm, and an outer diameter of 26 mm is polished with 280# and 180# sandpapers in turn, and then a thread with a depth of 0.4 mm is processed with a turning tool to obtain a threaded molybdenum tube shell;
[0052] Step 2: Disperse molybdenum powder with a particle size of 0.5 μm to 2.5 μm into an ethanol solution of polyvinyl butyral with a mass fraction of 3% and stir well to obtain a molybdenum powder slurry;
[0053] Step 3: Use centrifugal coating to coat the inner wall of the threaded molybdenum tube shell obtained in step 1 with the molybdenum powder slurry obtained in step 2 with a thickness of 0.8 mm, and then 3 / h atmosphere and then sintered to 1260°C for 2h to obtain a molybdenum tube shell having an ultrafine porous molybdenum layer, wherein the maximum pore size of the ultrafine porous molybdenum layer is 0.53 μm;
[0054] Step 4: The molybdenum tube shell with the ultrafine porous molybdenum layer obtained in step 3 is used as a tube shell, and then filled with mixed molybdenum powder formed by mixing molybdenum powder with a particle size of 0.5 μm to 2.5 μm and molybdenum powder with a particle size of 15 μm to 50 μm in a mass ratio of 2:1, and then placed in a cold isostatic pressing device for cold isostatic pressing at a pressure of 200 MPa and maintained for 30 seconds to obtain a cold isostatic pressed molybdenum tube shell;
[0055] Step 5: Place the cold isostatically pressed molybdenum shell obtained in step 4 under a hydrogen flow rate of 0.4 m 3 / h atmosphere to 1400°C for sintering to obtain a sintered molybdenum tube shell;
[0056] Step six, the inner wall of the sintered molybdenum tube shell obtained in step five is processed with a multi-step groove structure, each group of multi-step groove structures 4 includes 7 grooves, and the groove depth first gradually increases and then gradually decreases, to obtain a porous molybdenum composite heat pipe, the thickness of the ultrafine porous molybdenum layer 2 of the porous molybdenum composite heat pipe is 0.8 mm, the maximum pore size is 1.5 μm, the thickness of the porous molybdenum liquid wick 3 is 3.6 mm, the maximum pore size is 10.6 μm, and the depth of the groove structure is 0.8 mm to 3.4 mm.
[0057] After testing, it was found that the porous molybdenum composite heat pipe prepared in this embodiment was normally used at a working temperature of 1500K.
[0058] Example 4
[0059] This embodiment includes the following steps:
[0060] Step 1: The inner wall of a molybdenum tube with a length of 100 mm, a wall thickness of 2 mm, and an outer diameter of 21 mm is polished with 280# and 180# sandpapers in turn, and then a thread with a depth of 0.3 mm is processed with a turning tool to obtain a threaded molybdenum tube shell;
[0061] Step 2: Disperse molybdenum powder with a particle size of 0.5 μm to 2.5 μm into an ethanol solution of polyvinyl butyral with a mass fraction of 4% and stir well to obtain a molybdenum powder slurry;
[0062] Step 3: Use centrifugal coating to coat the inner wall of the threaded molybdenum tube shell obtained in step 1 with the molybdenum powder slurry obtained in step 2 with a thickness of 0.6 mm, and then 3 / h atmosphere and then sintered to 1230°C for 2h to obtain a molybdenum tube shell having an ultrafine porous molybdenum layer, wherein the maximum pore size of the ultrafine porous molybdenum layer is 0.9 μm;
[0063] Step 4: The molybdenum tube shell with the ultrafine porous molybdenum layer obtained in step 3 is used as a tube shell, and then filled with mixed molybdenum powder formed by mixing molybdenum powder with a particle size of 0.5 μm to 2.5 μm and molybdenum powder with a particle size of 15 μm to 50 μm in a mass ratio of 3:1, and then placed in a cold isostatic pressing device for cold isostatic pressing at a pressure of 160 MPa and maintained for 90 seconds to obtain a cold isostatic pressed molybdenum tube shell;
[0064] Step 5: Place the cold isostatically pressed molybdenum shell obtained in step 4 under a hydrogen flow rate of 0.3 m 3 / h atmosphere to 1300°C for sintering to obtain a sintered molybdenum tube shell;
[0065] Step six, the inner wall of the sintered molybdenum tube shell obtained in step five is processed with a multi-step groove structure, each group of multi-step groove structures 4 includes 9 grooves, and the groove depth first gradually increases and then gradually decreases, to obtain a porous molybdenum composite heat pipe, the thickness of the ultrafine porous molybdenum layer 2 of the porous molybdenum composite heat pipe is 0.6mm, the maximum pore size is 1.1μm, the thickness of the porous molybdenum liquid wick 3 is 3.7mm, the maximum pore size is 5.2μm, and the depth of the groove structure is 0.8mm~3.4mm.
[0066] After testing, it was found that the porous molybdenum composite heat pipe prepared in this embodiment was normally used at a working temperature of 1400K.
[0067] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A porous molybdenum composite heat pipe, It is characterized in that The porous molybdenum composite heat pipe is composed of a molybdenum tube shell (1), an ultrafine porous molybdenum layer (2) and a porous molybdenum liquid absorption core (3) with a multi-step groove structure (4) in sequence from the outside to the inside.
2. A porous molybdenum composite heat pipe according to claim 1, It is characterized in that The wall thickness of the molybdenum tube shell (1) is 1 mm to 2 mm, the thickness of the ultrafine porous molybdenum layer (2) is 0.5 mm to 0.8 mm, the pore size of the porous structure in the ultrafine porous molybdenum layer (2) is 0.5 μm to 1.5 μm, the thickness of the porous molybdenum liquid absorption core (3) is 3.6 mm to 3.8 mm, the pore size of the porous structure in the porous molybdenum liquid absorption core (3) is 5 μm to 25 μm, and the depth of the multi-step groove structure is 0.8 mm to 3.4 mm.
3. The porous molybdenum composite heat pipe according to claim 1, It is characterized in that The multi-step groove structure (4) is divided into a plurality of groups, each group of the multi-step groove structure (4) comprises 3 to 9 grooves, and the groove depth first gradually increases and then gradually decreases.
4. A method for preparing a porous molybdenum composite heat pipe according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: Step 1: Grind the inner wall of the molybdenum tube, and then process the threads to obtain a threaded molybdenum tube shell; Step 2: dispersing molybdenum powder into an ethanol solution of polyvinyl butyral and stirring the mixture to obtain a molybdenum powder slurry; Step 3: coating the inner wall of the threaded molybdenum tube shell obtained in step 1 with the molybdenum powder slurry obtained in step 2, and then sintering the inner wall under a hydrogen atmosphere to obtain a molybdenum tube shell having an ultrafine porous molybdenum layer; Step 4: The molybdenum tube shell with the ultrafine porous molybdenum layer obtained in step 3 is used as a tube shell, and then filled with mixed molybdenum powder, and then cold isostatically pressed to obtain a cold isostatically pressed molybdenum tube shell; Step 5, sintering the cold isostatically pressed molybdenum tube shell obtained in step 4 under a hydrogen atmosphere to obtain a sintered molybdenum tube shell; Step 6: Process the inner wall of the sintered molybdenum tube shell obtained in step 5 into a multi-step groove structure to obtain a porous molybdenum composite heat pipe.
5. The method according to claim 4, It is characterized in that The depth of the thread in step 1 is 0.3 mm to 0.5 mm.
6. The method according to claim 4, It is characterized in that The particle size of the molybdenum powder in step 2 is 0.5 μm to 2.5 μm, the mass fraction of polyvinyl butyral in the polyvinyl butyral ethanol solution is 3% to 5%, and the concentration of molybdenum powder in the molybdenum powder slurry is 0.25 g / mL to 0.35 g / mL.
7. The method according to claim 4, It is characterized in that The coating in step 3 is carried out by centrifugal coating, the coating thickness is 0.5 mm to 0.8 mm, the sintering temperature is 1200°C to 1260°C, the time is 2 h, and the hydrogen flow rate is 0.25 m 3 / h~0.4m 3 / h.
8. The method according to claim 4, It is characterized in that The mixed molybdenum powder in step 4 is formed by mixing molybdenum powder with a particle size of 0.5μm to 2.5μm and molybdenum powder with a particle size of 15μm to 50μm in a mass ratio of 1 to 3:
1. The cold isostatic pressing pressure is 160MPa to 200MPa, and the holding time is 30s to 150s.
9. The method according to claim 4, It is characterized in that The sintering temperature in step 5 is 1300°C to 1500°C, and the flow rate of hydrogen is 0.25m 3 / h~0.4m 3 / h.
Citation Information
Patent Citations
Composite liquid sucking core of toothed heat pipe and manufacturing method thereof
CN102359746A
Heat-tube composite liquid absorption core and preparation method for same
CN104075603A
Flat heat pipe composited groove type fluid suction core and preparation method thereof
CN106440898A
Hot metal high-temperature heat pipe
CN111473669A
Porous transport layer based on multiple micro and NANO sintered porous layers
CN113348269A