Method for testing mechanical performance of tubular test piece of electric wire

By attaching paper tape layers to both ends of the wire and using clamps to hold it, the problem of the test piece breaking near the clamps during the mechanical performance testing of the wire was solved, thus improving the testing efficiency and the accuracy of the results.

CN118937075APending Publication Date: 2024-11-12GOLD CUP ELECTRIC APP HENGYANG CABLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134224.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the mechanical performance testing of electrical wires, the specimens often break near the clamps, resulting in low testing efficiency and inaccurate results.

Method used

Adhesive paper tape is pasted on both ends of the wire, and the part with the adhesive paper tape is clamped with a clamp and slowly pulled along the axis until it breaks. The maximum tensile force and elongation at break are measured.

Benefits of technology

This effectively prevents the specimen from breaking near the clamp, improves testing efficiency, and ensures the accuracy and reliability of the test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937075A_ABST
    Figure CN118937075A_ABST
Patent Text Reader

Abstract

The invention discloses an electric wire tubular test piece mechanical property test method, which comprises the following steps: cutting a to-be-tested electric wire with a certain length, and respectively pasting at least one paper adhesive tape layer at two ends of the to-be-tested electric wire; a tension tester is arranged on the outer side of the to-be-tested wire, and chucks of the tension tester are used for correspondingly clamping the parts, pasted with the paper adhesive tape layers, of the two ends of the to-be-tested wire respectively; slowly pulling the two chucks along the axial direction of the to-be-tested wire until the to-be-tested wire is broken; the maximum tensile force is measured and recorded in the test period, then the tensile strength and the elongation at break are calculated, and after experimental comparison, it is obtained that all experimental group test pieces can effectively prevent the tubular test pieces from being broken near a chuck, so that re-testing is not needed, and then the detection efficiency is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of wire and cable detection, and more specifically, relates to a method for testing the mechanical properties of a wire tubular specimen. Background Art

[0002] The mechanical performance indicators of the wires need to be tested. At present, when doing mechanical performance tests, the test piece is generally in direct contact with the fixture. The experimental group has verified that when tracking the mechanical properties of low-smoke halogen-free flame-retardant polyolefin insulated wires, there is an 80% probability that the test piece will break near the clamp. According to the standard requirements, re-testing is required, and the clamp will also break during the re-testing, which greatly affects the detection efficiency and results. Summary of the invention

[0003] The main purpose of the present invention is to provide a method for testing the mechanical properties of a wire tubular specimen, which can improve the detection efficiency and thereby ensure the detection results.

[0004] To achieve the above object, the technical solution of the present invention is:

[0005] A method for testing the mechanical properties of a tubular wire specimen comprises the following steps: cutting a certain length of wire to be tested, and pasting at least one paper tape layer on both ends of the wire to be tested; arranging a tensile testing machine on the outside of the wire to be tested, and using the clamps of the tensile testing machine to respectively clamp the parts of the wire to be tested at both ends pasted with the paper tape layer; slowly pulling the two clamps along the axial direction of the wire to be tested until the wire to be tested breaks; measuring and recording the maximum tensile force during the test, and then calculating the tensile strength and elongation at break.

[0006] In a specific embodiment of the present invention, the paper tape layer is arranged along the axial direction of the wire to be tested, and when the clamp clamps the wire to be tested, the paper tape layer is exposed outside the clamp.

[0007] In a specific embodiment of the present invention, the length of the paper tape layer exposed from the clamping head is in the range of 5-10 mm.

[0008] In a specific embodiment of the present invention, the thickness of the paper adhesive tape layer is 0.12-0.27 mm.

[0009] In a specific embodiment of the present invention, the wire to be tested should be placed in an environment with a temperature of 18° C.-28° C. for at least 3 hours before the experiment.

[0010] In a specific embodiment of the present invention, the test requires that the wire to be tested be stored for at least 16 hours after the insulation and sheathing materials are extruded or vulcanized (or cross-linked).

[0011] In a specific embodiment of the present invention, the cut length of the wire to be tested is 50-85 mm, and the wire to be tested is a low-smoke, halogen-free, flame-retardant polyolefin insulated wire.

[0012] In a specific embodiment of the present invention, the moving speed of the two chucks is maintained at 200-300 mm / min.

[0013] In a specific embodiment of the present invention, the chuck is a self-tightening chuck or a non-self-tightening chuck.

[0014] One of the above technical solutions of the present invention has at least one of the following advantages or beneficial effects:

[0015] After cutting off a certain length of the wire to be tested, the present invention pastes at least one layer of paper tape on both ends of the wire to be tested, and then uses the chucks of the tensile testing machine to respectively clamp the parts of the wire to be tested with the paper tape layers, and slowly pulls the two chucks along the axial direction of the wire to be tested. After experimental comparison, it is found that each experimental group of test pieces can effectively avoid the tubular test pieces from breaking near the chucks, so there is no need to re-test, thereby significantly improving the detection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The present invention is further described below in conjunction with the accompanying drawings and embodiments;

[0017] Figure 1 is a clamping state diagram of an embodiment of the present invention;

[0018] Figure 2 is a front view of the wire to be tested after the paper tape layer is attached to one embodiment of the present invention;

[0019] Figure 3 It is a cross-sectional view along the AA direction of one embodiment of the present invention. DETAILED DESCRIPTION

[0020] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements having the same or similar functions from beginning to end. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0021] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, front, back, left, right, etc., and orientations or positional relationships indicated are based on the orientations or positional relationships shown in the accompanying drawings, and are merely simplified descriptions for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0022] In the description of the present invention, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed" etc. are understood as not including the number itself, and "above", "below", "within" etc. are understood as including the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0023] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more features.

[0024] In the description of the present invention, it should be noted that, unless otherwise clearly stipulated and limited, the term "connection" should be understood in a broad sense. For example, it can be a fixed connection or a movable connection, a detachable connection or a non-detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, and it can be internal connection between two elements, indirect connection, or an interactive relationship between two elements.

[0025] The following disclosure provides many different embodiments or examples for implementing different solutions of the present invention.

[0026] Reference Figures 1 to 3 As shown, a method for testing the mechanical properties of a tubular wire specimen includes the following steps: first, a certain length of wire to be tested is cut, the cut length is 50-85 mm, and the wire to be tested is a low-smoke, halogen-free, flame-retardant polyolefin insulated wire;

[0027] Furthermore, before the experiment, the wire to be tested is placed in an environment with a temperature of 18°C-28°C for at least 3 hours, and the wire to be tested needs to be stored for at least 16 hours after the insulation and sheath materials are extruded or vulcanized (or cross-linked), and at least one layer of paper tape 1 is pasted on both ends of the wire to be tested. Figure 3 As shown, the thickness of the paper adhesive tape layer 1 is selected to be between 0.12-0.27 mm;

[0028] Further, a tensile testing machine is arranged on the outside of the wire to be tested, such as Figure 1 As shown, the clamp 2 of the tensile testing machine is used to clamp the parts of the two ends of the wire to be tested with the paper tape layer 1 respectively, and the paper tape layer 1 is arranged along the axial direction of the wire to be tested. When the clamp 2 clamps the wire to be tested, the paper tape layer 1 is exposed from the clamp 2, and the length of the paper tape layer 1 exposed from the clamp 2 is further set to be in the range of 5-10mm;

[0029] Further, the two clamps 2 are slowly pulled along the axial direction of the wire to be tested until the wire to be tested breaks, and the moving speed of the two clamps 2 is maintained at 200-300 mm / min;

[0030] Finally, the maximum tensile force was measured and recorded during the test, and at least 4 valid data were obtained to calculate the tensile strength and elongation at break.

[0031] The specific steps for conducting the tensile test are as follows: first, the test should be carried out at a temperature of (23±5)℃. If there is any doubt about the thermoplastic insulating material, the test should be carried out at a temperature of (23±2)℃.

[0032] The spacing and moving speed between the chucks 2 are further set. The chucks 2 of the tensile testing machine can be self-tightening chucks or non-self-tightening chucks. The total spacing between the chucks 2 varies according to the shape of the specimen. For example, the dumbbell specimen is 34mm-50mm, the tubular specimen is 50mm when tested with a self-tightening chuck, and the tubular specimen is 85mm when tested with a non-self-tightening chuck.

[0033] The moving speed of the clamp 2 is further set to (250±50) mm / min, except for PE and PP insulation. In case of doubt, the moving speed should be (25±5) mm / min. If PE and PP insulation, or insulation containing these materials, the moving speed should be (25±5) mm / min. However, when conducting routine tests, the moving speed is allowed to be (250±50) mm / min and below.

[0034] Finally, measure and record the maximum tensile force during the test, and at the same time measure the distance between the two marking lines when breaking on the same specimen. The test results of any specimen that breaks at clamp 2 should be invalidated. In this case, at least 4 valid data are required to calculate the tensile strength and elongation at break, otherwise the test should be repeated.

[0035] In one embodiment of the present invention, regarding the test results and the method of expression, it is necessary to record the maximum tensile stress when the specimen is stretched to fracture, and the percentage of the increment of the marked distance when the specimen is stretched to fracture and the marked distance of the unstretched specimen, so as to determine the middle value of the test result.

[0036] Using this wire tubular specimen mechanical property test method, after conducting four groups of control experiments, the following control table can be obtained:

[0037] Table 1

[0038]

[0039] As shown in Table 1, in the experimental group where no paper tape was pasted on both ends of the tested wire, 80% of the test pieces had fracture locations near the clamp 2;

[0040] At least one layer of paper tape layer 1 is axially attached to both ends of the wire to be tested, and when the clamp 2 is provided to clamp the wire to be tested, the length of the paper tape layer 1 exposed from the clamp 2 is in the range of 5-10 mm. After the test pieces of each experimental group are broken, they are broken within the marking line. This can effectively avoid the tubular test piece from breaking near the clamp 2 without the need for re-testing, which significantly improves the detection efficiency. In addition, the elongation at break of this group of wires is also greatly improved compared with the experimental group where no paper tape is attached to both ends.

[0041] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for testing the mechanical properties of a tubular wire specimen, characterized in that: The steps include: 1) Cut a certain length of the wire to be tested, and stick at least one layer of paper tape (1) on both ends of the wire to be tested; 2) Arranging a tensile testing machine on the outside of the wire to be tested, and using the clamp (2) of the tensile testing machine to respectively clamp the parts of the two ends of the wire to be tested on which the paper tape layer (1) is pasted; 3) slowly pulling the two clamps (2) along the axial direction of the wire to be tested until the wire to be tested breaks; 4) Measure and record the maximum tensile force during the test, and then calculate the tensile strength and elongation at break.

2. The method for testing the mechanical properties of a tubular wire specimen according to claim 1, characterized in that: The paper tape layer (1) is arranged along the axial direction of the wire to be tested, and when the clamp (2) clamps the wire to be tested, the paper tape layer (1) is exposed outside the clamp (2).

3. The method for testing the mechanical properties of a tubular wire specimen according to claim 2, characterized in that: The length of the paper tape layer (1) exposed from the clamp (2) is in the range of 5-10 mm.

4. The method for testing mechanical properties of a tubular wire specimen according to claim 3, characterized in that: The thickness of the paper adhesive tape layer (1) is 0.12-0.27 mm.

5. The method for testing mechanical properties of a tubular wire specimen according to claim 1, characterized in that: The wire to be tested should be placed in an environment with a temperature of 18℃-28℃ for at least 3 hours before the experiment.

6. The method for testing mechanical properties of a tubular wire specimen according to claim 1, characterized in that: The test requires that the wire to be tested be stored for at least 16 hours after the insulation and sheath materials are extruded or vulcanized (or cross-linked).

7. The method for testing the mechanical properties of a tubular wire specimen according to claim 1, characterized in that: The cut length of the wire to be tested is 50-85mm, and the wire to be tested is a low-smoke, halogen-free, flame-retardant polyolefin insulated wire.

8. The method for testing the mechanical properties of a tubular wire specimen according to claim 1, characterized in that: The moving speed of the two chucks (2) is maintained at 200-300 mm / min.

9. The method for testing mechanical properties of a tubular wire specimen according to claim 8, characterized in that: The chuck (2) is a self-tightening chuck or a non-self-tightening chuck.