Device and method for detecting residual solvent in cigarette packaging material

By passing gas on the upper and lower surfaces of the cigarette packaging material to detect the solvent content and change rate, the problem of residual solvent in the cigarette packaging material affecting quality is solved, and the effect of accurate judgment and improved process is achieved.

CN118937600APending Publication Date: 2024-11-12CHINA TOBACCO HENAN IND CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411309536.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The residual solvent in the cigarette packaging material will affect the odor and taste of the cigarette, and will be easily contaminated during processing, storage and transportation. It is difficult for the prior art to effectively distinguish the source of residual solvents.

Method used

A detection device and method for residual solvent in cigarette packaging materials was designed. By passing gas into the upper and lower surfaces of the packaging materials, the solvent content and content change rate in the gas are detected, and whether the solvent comes from the preparation process or stored. /Contamination during transportation.

Benefits of technology

Able to accurately determine the source of solvents in packaging materials, help improve preparation, storage and transportation processes, and ensure the improvement of cigarette quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937600A_ABST
    Figure CN118937600A_ABST
Patent Text Reader

Abstract

The invention discloses a device and method for detecting residual solvents in cigarette packaging materials, and the device comprises a first pressing plate and a second pressing plate which are oppositely arranged from bottom to top, the bottom surface of the first pressing plate is provided with a first groove, and the left side of the first groove in the first pressing plate is provided with a first air inlet channel; a first air outlet channel is formed in the right side of the first groove in the first pressing plate; a second groove is formed in the top face of the second pressing plate, a second air inlet channel is formed in the left side of the second groove in the second pressing plate, and a second air outlet channel is formed in the right side of the second groove in the second pressing plate. A preset gap is formed between the first pressing plate and the second pressing plate and used for containing a base material of a packaging material, the opening edge of the first groove presses the upper surface of the base material, and the opening edge of the second groove presses the lower surface of the base material. According to the detection device and the detection method for the residual solvent in the cigarette packaging material, whether the residual solvent in the packaging material is residual in the preparation process or polluted in the storage or transportation process can be distinguished through detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of tobacco packaging, and more specifically, to a detection device and a detection method for residual solvent in cigarette packaging materials. Background Art

[0002] In the process of cigarette rolling, different packaging materials are often needed for rolling or packaging. The residual solvents in the packaging materials used for cigarettes will affect the smell or taste of the cigarettes. Therefore, the solvents in the packaging materials of cigarettes need to be strictly controlled.

[0003] During the manufacturing, transportation and storage of packaging materials, solvents will remain in the packaging materials. During transportation or storage, the packaging materials may also be contaminated by solvents. The residual solvents in the packaging materials may contaminate or affect the quality of cigarettes when they are packaged. Organic solvents are often used in the processing of packaging materials, so that the packaging materials contain volatile organic solvents, such as ethanol, isopropanol, ethyl acetate, methanol, acetone, benzene, toluene, ethylbenzene, etc. Some solvents evaporate during the processing, but there are still residues. At the same time, during the storage or transportation of packaging materials, they may be affected by the surrounding environment, causing the solvents in the surrounding environment to contaminate the packaging materials.

[0004] Therefore, there is an urgent need for a detection device and method for residual solvents in cigarette packaging materials. Summary of the invention

[0005] The purpose of the present invention is to provide a detection device and method for residual solvents in cigarette packaging materials to solve the above-mentioned problems in the prior art and to be able to identify through detection whether the residual solvents in the packaging materials are residuals from the preparation process or contaminated during storage or transportation.

[0006] The present invention provides a detection device for residual solvent in cigarette packaging materials, which includes: a first pressing plate and a second pressing plate arranged opposite to each other from bottom to top, a first groove is provided on the bottom surface of the first pressing plate, a first air inlet is provided on the left side of the first groove on the first pressing plate, and a first air outlet is provided on the right side of the first groove on the first pressing plate;

[0007] A second groove is formed on the top surface of the second pressing plate, a second air inlet is formed on the left side of the second groove on the second pressing plate, and a second air outlet is formed on the right side of the second groove on the second pressing plate;

[0008] A preset gap is formed between the first pressing plate and the second pressing plate for placing a substrate of packaging material, the opening edge of the first groove presses the upper surface of the substrate, and the opening edge of the second groove presses the lower surface of the substrate.

[0009] The detection device for residual solvent in cigarette packaging material as described above, wherein, preferably, the left side wall of the first groove is provided with a first upper opening; the lower edge of the first upper opening is provided with a first upper accommodating cavity, and a movable first upper adjusting plate is provided in the first upper accommodating cavity; the right side wall of the first groove is provided with a second upper opening, the lower edge of the second upper opening is provided with a second upper accommodating cavity, and a movable second upper adjusting plate is provided in the first upper accommodating cavity;

[0010] A first lower opening is formed on the left side wall of the second groove, a first lower accommodating chamber is provided on the upper edge of the first lower opening, and a movable first lower adjustment plate is provided in the first lower accommodating chamber; a second lower opening is formed on the right side wall of the second groove, a second lower accommodating chamber is provided on the upper edge of the second lower opening, and a movable second lower adjustment plate is provided in the first lower accommodating chamber.

[0011] The detection device for residual solvent in cigarette packaging material as described above, wherein preferably, the first upper opening and the second upper opening have the same shape and size, and the first upper opening and the second upper opening are symmetrically arranged about the middle position of the first groove;

[0012] The first lower opening and the second lower opening have the same shape and size, and the first lower opening and the second lower opening are symmetrically arranged about a middle position of the second groove.

[0013] The detection device for residual solvent in cigarette packaging material as described above, wherein, preferably, the bottom surface of the first upper adjusting plate is provided with a first elastic layer, and the first elastic layer on the portion of the first upper adjusting plate extending from the first upper accommodating cavity abuts against the upper surface of the substrate; the bottom surface of the second upper adjusting plate is provided with a second elastic layer, and the second elastic layer on the portion of the second upper adjusting plate extending from the second upper accommodating cavity abuts against the upper surface of the substrate;

[0014] A third elastic layer is arranged on the top surface of the first lower adjustment plate, and the third elastic layer on the portion of the first lower adjustment plate extending from the first lower accommodating cavity stops against the lower surface of the substrate; a fourth elastic layer is arranged on the top surface of the second lower adjustment plate, and the fourth elastic layer on the portion of the second lower adjustment plate extending from the second lower accommodating cavity stops against the lower surface of the substrate.

[0015] As described above, the device for detecting residual solvents in cigarette packaging materials, wherein preferably, scale lines are provided on the first upper adjusting plate, the second upper adjusting plate, the first lower adjusting plate and the second lower adjusting plate.

[0016] The device for detecting residual solvents in cigarette packaging materials as described above, wherein preferably, the diameters of the first air inlet, the first air outlet, the second air inlet and the second air outlet are the same; the opening of the first groove and the opening of the second groove are arranged opposite to each other, and the first groove and the second groove have the same shape and size; the first air inlet and the first air outlet are arranged symmetrically about the first groove; and the second air inlet and the second air outlet are arranged symmetrically about the second groove.

[0017] The present invention provides a method for detecting residual solvents in cigarette packaging materials, which comprises:

[0018] introducing gas through the first air inlet and the second air inlet respectively;

[0019] The gas introduced through the first gas inlet flows over the upper surface of the substrate, the solvent overflows from the upper surface of the substrate along with the gas, and the gas flows out from the first gas outlet;

[0020] The gas introduced through the second gas inlet flows through the lower surface of the substrate, the solvent overflows from the lower surface of the substrate along with the gas, and the gas flows out from the second gas outlet;

[0021] Respectively detecting the content and content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet;

[0022] The source of the residual solvent in the packaging material is determined based on whether the content and the content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet are consistent.

[0023] The method for detecting residual solvents in cigarette packaging materials as described above, wherein preferably, the gas introduced into the first air inlet and the second air inlet includes an inert gas, and the solvent in the gas flowing out from the first air outlet and the second air outlet includes at least one of methanol, ethanol, propanol, benzene, toluene, xylene and acetone.

[0024] The method for detecting residual solvent in cigarette packaging material as described above, wherein preferably, judging the source of the residual solvent in the packaging material based on whether the content and content change rate of the solvent in the gas flowing out of the first air outlet and the second air outlet are consistent, specifically includes:

[0025] If the content and content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet of the substrate are consistent, the solvent in the substrate is residual during preparation;

[0026] If at least one of the content and the content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet of the substrate is inconsistent, the solvent in the substrate is contaminated during storage and transportation.

[0027] The above-mentioned method for detecting residual solvents in cigarette packaging materials, wherein, preferably, the method for detecting residual solvents in cigarette packaging materials further comprises:

[0028] For the same batch of packaging material substrates, different areas are selected as sample substrates for testing. The source of the residual solvent in the packaging material is determined based on whether the content and content change rate of the solvent in the gas flowing through the upper and lower surfaces of the substrate in each area are consistent, including:

[0029] If the solvent content and content change rate of the gas flowing out of the first gas outlet and the second gas outlet corresponding to each region of the substrate are consistent, the solvent in the substrate is residual during preparation;

[0030] If at least one of the content and content change rate of the solvent in the gas flowing through the upper surface and the lower surface of the substrate in different areas is inconsistent, the solvent in the substrate is contaminated during storage and transportation.

[0031] The present invention provides a detection device and method for residual solvent in cigarette packaging materials. Gas is introduced through a first air inlet and a second air inlet to make the gas flow through the upper surface and the lower surface of a substrate. The solvent overflows from the upper surface of the substrate along with the gas, and the gas flows out from a first air outlet and a second air outlet. By detecting the content and content change rate of the solvent in the gas flowing out from the first air outlet and the second air outlet, it can be determined whether the residual solvent in the packaging material is a residue in the preparation process or contaminated during storage or transportation, so as to improve the preparation, storage, transportation methods and process technology of the packaging material. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described below with reference to the accompanying drawings, in which:

[0033] Figure 1 A schematic structural diagram of an embodiment of a detection device for residual solvents in cigarette packaging materials provided by the present invention;

[0034] Figure 2 This is a flow chart of an embodiment of a method for detecting residual solvents in cigarette packaging materials provided by the present invention.

[0035] Explanation of the figure markings: 10-first pressing plate, 11-first groove, 12-first air inlet, 13-first air outlet, 14-first upper adjusting plate, 15-second upper adjusting plate, 20-second pressing plate, 21-second groove, 22-second air inlet, 23-second air outlet, 24-first lower adjusting plate, 25-second lower adjusting plate, 30-substrate. DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present disclosure will now be described in detail with reference to the accompanying drawings. The description of the exemplary embodiments is merely illustrative and is in no way intended to limit the present disclosure and its application or use. The present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. These embodiments are provided to make the present disclosure thorough and complete and to fully express the scope of the present disclosure to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the components and steps, the composition of the materials, the numerical expressions and the numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary and not as limiting.

[0037] The words "first", "second" and similar words used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different parts. The words "include" or "comprises" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements. "Up", "down" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0038] In the present disclosure, when a specific component is described as being located between a first component and a second component, there may or may not be an intermediate component between the specific component and the first component or the second component. When a specific component is described as being connected to other components, the specific component may be directly connected to the other components without an intermediate component, or may not be directly connected to the other components but have an intermediate component.

[0039] All terms (including technical terms or scientific terms) used in the present disclosure have the same meanings as those understood by ordinary technicians in the field to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, such as general dictionaries, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0040] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0041] like Figure 1 As shown, the detection device for residual solvent in cigarette packaging material provided in this embodiment comprises: a first pressing plate 10 and a second pressing plate 20 arranged opposite to each other from bottom to top, a first groove 11 is provided on the bottom surface of the first pressing plate 10, a first air inlet 12 is provided on the left side of the first groove 11 on the first pressing plate 10, and a first air outlet 13 is provided on the right side of the first groove 11 on the first pressing plate 10;

[0042] A second groove 21 is formed on the top surface of the second pressing plate 20, a second air inlet 22 is formed on the left side of the second groove 21 on the second pressing plate 20, and a second air outlet 23 is formed on the right side of the second groove 21 on the second pressing plate 20;

[0043] A preset gap is formed between the first pressing plate 10 and the second pressing plate 20 for placing a substrate 30 of the packaging material. The opening edge of the first groove 11 presses the upper surface of the substrate 30 , and the opening edge of the second groove 21 presses the lower surface of the substrate 30 .

[0044] The first pressing plate 10 and the second pressing plate 20 may be metal plates or glass plates, or may be transparent plates.

[0045] Furthermore, the opening of the first groove 11 is arranged opposite to the opening of the second groove 21, and the first groove 11 and the second groove 21 have the same shape and size. By introducing gas into the first groove 11 and the second groove 21, the gas can cause the solvent on the surface of the substrate to overflow the substrate 30 and flow out along with the gas.

[0046] Further, the diameters of the first air inlet 12, the first air outlet 13, the second air inlet 22 and the second air outlet 23 are the same. The first air inlet 12 and the first air outlet 13 are symmetrically arranged about the first groove 11; the second air inlet 22 and the second air outlet 23 are symmetrically arranged about the second groove 21.

[0047] In operation, the gas is introduced from the first air inlet 12, flows through the upper surface of the substrate 30 when passing through the first groove 11, and flows out from the first air outlet 13 on the right side of the first groove 11, which can be conducive to carrying away the solvent in the substrate 30 of the packaging material; correspondingly, the gas is introduced from the second air inlet 22, flows through the lower surface of the substrate 30 when passing through the second groove 21, and flows out from the second air outlet 23 on the right side of the second groove 21, which can be conducive to carrying away the solvent in the substrate 30 of the packaging material. The content of the solvent in the gas flowing out from the first air outlet 13 and the second air outlet 23 can be detected to determine whether the solvent, the content and the content change rate are the same. If the solvent in the substrate 30 is residual during preparation, the content and content change rate of the solvent in the gas flowing through the upper and lower surfaces of the substrate 30 are the same; if the solvent in the substrate 30 is contaminated during storage and transportation, the content and content change rate of the solvent in the gas flowing through the upper and lower surfaces of the substrate 30 are different.

[0048] Furthermore, a first upper opening is provided on the left side wall of the first groove 11; a first upper accommodating cavity is provided on the lower edge of the first upper opening, and a movable first upper adjusting plate 14 is provided in the first upper accommodating cavity; a second upper opening is provided on the right side wall of the first groove 11, a second upper accommodating cavity is provided on the lower edge of the second upper opening, and a movable second upper adjusting plate 15 is provided in the first upper accommodating cavity. Specifically, the first upper opening and the second upper opening have the same shape and size, and the first upper opening and the second upper opening are symmetrically arranged about the middle position of the first groove 11. The size of the opening of the first groove 11 can be adjusted by moving the first upper adjusting plate 14 and the second upper adjusting plate 15, and the first upper adjusting plate 14 and the second upper adjusting plate 15 can be covered on the upper surface of the substrate 30, so that the area size of the exposed area of ​​the upper surface of the substrate 30 is different.

[0049] Furthermore, a first elastic layer is provided on the bottom surface of the first upper adjustment plate 14, and the first elastic layer on the portion of the first upper adjustment plate 14 extending from the first upper accommodating cavity abuts against the upper surface of the substrate 30, so that the upper surface of the substrate 30 is not exposed; a second elastic layer is provided on the bottom surface of the second upper adjustment plate 15, and the second elastic layer on the portion of the second upper adjustment plate 15 extending from the second upper accommodating cavity abuts against the upper surface of the substrate 30, so that the area on the upper surface of the substrate 30 that the adjustment plate contacts is not exposed.

[0050] Further, a first lower opening is formed on the left side wall of the second groove 21, a first lower accommodating cavity is formed on the upper edge of the first lower opening, and a movable first lower adjusting plate 24 is formed in the first lower accommodating cavity; a second lower opening is formed on the right side wall of the second groove 21, a second lower accommodating cavity is formed on the upper edge of the second lower opening, and a movable second lower adjusting plate 25 is formed in the first lower accommodating cavity. The first lower opening and the second lower opening have the same shape and size, and the first lower opening and the second lower opening are symmetrically arranged about the middle position of the second groove 21. By moving the first lower adjusting plate 24 and the second lower adjusting plate 25, the size of the opening of the second groove 21 can be adjusted, and the first lower adjusting plate 24 and the second lower adjusting plate 25 can be covered on the lower surface of the substrate 30, so that the area size of the exposed area of ​​the lower surface of the substrate 30 is different.

[0051] A third elastic layer is provided on the top surface of the first lower adjustment plate 24, and the third elastic layer on the portion of the first lower adjustment plate extending from the first lower accommodating cavity abuts against the lower surface of the substrate 30, so that the lower surface of the substrate 30 is not exposed; a fourth elastic layer is provided on the top surface of the second lower adjustment plate 25, and the fourth elastic layer on the portion of the second lower adjustment plate extending from the second lower accommodating cavity abuts against the lower surface of the substrate 30, so that the area where the adjustment plate contacts the lower surface of the substrate 30 is not exposed.

[0052] The first upper adjusting plate 14 , the second upper adjusting plate 15 , the first lower adjusting plate 24 and the second lower adjusting plate 25 are provided with scale lines to facilitate judging the extended length and further judging the surface of the covered substrate.

[0053] By moving the first upper adjustment plate 14, the second upper adjustment plate 15, the first lower adjustment plate 24 and the second lower adjustment plate 25, the size of the exposed surface area of ​​the substrate 30 can be changed, and different areas or regions of the surface of the substrate 30 can be exposed as needed to detect the desired area or region, which can be suitable for detecting substrates 30 of packaging materials of different sizes.

[0054] The device for detecting residual solvents in cigarette packaging materials provided in an embodiment of the present invention introduces gas through a first air inlet and a second air inlet, causing the gas to flow through the upper and lower surfaces of a substrate, and the solvent overflows from the upper surface of the substrate along with the gas, and the gas flows out from a first air outlet and a second air outlet. By detecting the content and content change rate of the solvent in the gas flowing out from the first air outlet and the second air outlet, it can be determined whether the residual solvent in the packaging material is a residue from the preparation process or contaminated during storage or transportation, so as to improve the preparation, storage, transportation methods, and process technology of the packaging material.

[0055] like Figure 2 As shown, the detection method for residual solvents in cigarette packaging materials provided in this embodiment includes the following steps in actual implementation:

[0056] Step S1 , introducing gas through the first air inlet 12 and the second air inlet 22 respectively.

[0057] The gas introduced into the first air inlet 12 and the second air inlet 22 is an inert gas, such as nitrogen, argon, helium, etc., or an organic solvent capable of dissolving the solvent to be detected, and the temperature of the gas can be 30° C.- 60° C. In some embodiments of the present invention, the introduced gas can be a non-oxidizing gas, which does not contain oxygen, ozone, etc.

[0058] Step S2 , the gas introduced through the first gas inlet 12 flows over the upper surface of the substrate 30 , the solvent overflows from the upper surface of the substrate 30 along with the gas, and the gas flows out from the first gas outlet 13 .

[0059] Step S3 , the gas introduced through the second gas inlet 22 flows through the lower surface of the substrate 30 , the solvent overflows from the lower surface of the substrate 30 along with the gas, and the gas flows out from the second gas outlet 23 .

[0060] By flowing gas over the upper and lower surfaces of the substrate 30 , the flow rate, temperature, and pressure of the gas flowing over the upper and lower surfaces of the substrate 30 are the same, so that the solvent flowing over the upper and lower surfaces of the substrate is the same.

[0061] In step S2 and step S3, the solvent in the gas flowing out from the first gas outlet 13 and the second gas outlet 23 includes at least one of methanol, ethanol, propanol, benzene, toluene, xylene and acetone.

[0062] Step S4, respectively detecting the content and content change rate of the solvent in the gas flowing out of the first gas outlet 13 and the second gas outlet 23.

[0063] In a specific implementation, detection may be performed once every certain period of time (for example, one month), and the content of the solvent in the gas and the rate of change of the content at different times may be obtained.

[0064] Step S5: judging the source of the residual solvent in the packaging material according to whether the content and content change rate of the solvent in the gas flowing out from the first gas outlet 13 and the second gas outlet 23 are consistent.

[0065] In one embodiment of the method for detecting residual solvents in cigarette packaging materials of the present invention, step S5 may specifically include:

[0066] Step S51 : If the content and content change rate of the solvent in the gas flowing out from the first gas outlet 13 and the second gas outlet 23 of the substrate 30 are consistent, the solvent in the substrate 30 is residual during preparation.

[0067] Step S52: If at least one of the content and the content change rate of the solvent in the gas flowing out of the first gas outlet 13 and the second gas outlet 23 of the substrate 30 is inconsistent, the solvent in the substrate 30 is contaminated during storage and transportation.

[0068] The present invention can identify whether the solvent in the base material 30 of the packaging material is residual during preparation or contaminated during storage and transportation, so as to improve the preparation, storage, transportation method and process technology of the packaging material.

[0069] Furthermore, in some embodiments of the present invention, the method for detecting residual solvents in cigarette packaging materials further comprises:

[0070] Step S6: For the same batch of packaging material substrates, different areas are selected as sample substrates for testing, and the source of the residual solvent in the packaging material is determined based on whether the content and content change rate of the solvent in the gas flowing through the upper and lower surfaces of the substrate in each area are consistent.

[0071] Specifically, for the substrate 30 of the packaging material of the same batch, different regions are selected as sample substrates and tested through steps S1 to S4.

[0072] In one embodiment of the method for detecting residual solvents in cigarette packaging materials of the present invention, step S6 may specifically include:

[0073] Step S61: If the solvent content and content change rate of the gases flowing out of the first gas outlet 13 and the second gas outlet 23 corresponding to each region of the substrate are consistent, the solvent in the substrate is residual during preparation.

[0074] Step S62: If at least one of the content and content change rate of the solvent in the gas flowing through the upper surface and the lower surface of the substrate in different regions is inconsistent, the solvent in the substrate is contaminated during storage and transportation.

[0075] Furthermore, in some embodiments of the present invention, the method for detecting residual solvents in cigarette packaging materials further comprises:

[0076] Step S7: preparing a comparison sample.

[0077] In one embodiment of the method for detecting residual solvents in cigarette packaging materials of the present invention, step S7 may specifically include:

[0078] Step S71 , cutting out packaging materials to be inspected as initial packaging materials.

[0079] Step S72, placing the initial packaging material in an inert gas flow at 10° C.-30° C. for 10 h-24 h.

[0080] Step S73, placing the initial packaging material in a vacuum environment at 10° C.-30° C. for 10 h-20 h.

[0081] Step S74, placing the initial packaging material in a solvent, solvent gas or solvent solution for 4 h to 16 h.

[0082] Step S75: After taking out the initial packaging material, perform drying treatment.

[0083] Specifically, if the initial packaging material is placed in a solution in step S74, the initial packaging material is dried at 10°C-30°C, and finally, a dried initial packaging material is obtained.

[0084] Step S76: Acquire solvent change data of the initial packaging material.

[0085] Step S77, introducing gas through the first air inlet 12, causing the gas to flow through the upper surface of the substrate of the initial packaging material, the solvent overflows from the upper surface of the substrate of the initial packaging material along with the gas, and the gas flows out from the first air outlet 13; at the same time, introducing gas through the second air inlet 22, causing the gas to flow through the lower surface of the substrate of the initial packaging material, the solvent overflows from the lower surface of the substrate along with the gas, and the gas flows out from the second air outlet 23;

[0086] Step S78, respectively detect the content and content change rate of the solvent in the gas flowing out of the first gas outlet 13 and the second gas outlet 23. The detection can be performed once at a certain interval to obtain the content and content change rate of the solvent in the gas at different times.

[0087] Among them, the detection method for the substrate of the initial packaging material is the same as the detection method for the substrate of the packaging material. By comparing the solvent content and content change rate detected from the substrate of the packaging material with the solvent content and content change rate detected from the substrate of the initial packaging material, the change of the solvent in the substrate can be judged.

[0088] The method for detecting residual solvents in cigarette packaging materials provided by an embodiment of the present invention introduces gas through a first air inlet and a second air inlet, causing the gas to flow through the upper and lower surfaces of a substrate, and the solvent overflows the substrate from the upper surface of the substrate along with the gas, and the gas flows out from a first air outlet and a second air outlet. By detecting whether the content and content change rate of the solvent in the gas flowing out from the first air outlet and the second air outlet are consistent, it is possible to distinguish whether the residual solvent in the packaging material is a residue from the preparation process or contaminated during storage or transportation, so as to improve the preparation, storage, transportation methods, and process technology of the packaging material.

[0089] So far, various embodiments of the present disclosure have been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.

[0090] Although some specific embodiments of the present disclosure have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present disclosure. The scope of the present disclosure is defined by the appended claims.

Claims

1. A detection device for residual solvent in cigarette packaging materials, characterized in that: include: A first pressing plate and a second pressing plate are arranged opposite to each other from bottom to top, wherein a first groove is provided on the bottom surface of the first pressing plate, a first air inlet is provided on the left side of the first groove on the first pressing plate, and a first air outlet is provided on the right side of the first groove on the first pressing plate; A second groove is formed on the top surface of the second pressing plate, a second air inlet is formed on the left side of the second groove on the second pressing plate, and a second air outlet is formed on the right side of the second groove on the second pressing plate; A preset gap is formed between the first pressing plate and the second pressing plate for placing a substrate of packaging material, the opening edge of the first groove presses the upper surface of the substrate, and the opening edge of the second groove presses the lower surface of the substrate.

2. The detection device for residual solvent in cigarette packaging material according to claim 1, characterized in that: A first upper opening is formed on the left side wall of the first groove; a first upper accommodating cavity is formed on the lower edge of the first upper opening, and a movable first upper adjusting plate is disposed in the first upper accommodating cavity; a second upper opening is formed on the right side wall of the first groove, a second upper accommodating cavity is formed on the lower edge of the second upper opening, and a movable second upper adjusting plate is disposed in the first upper accommodating cavity; A first lower opening is formed on the left side wall of the second groove, a first lower accommodating chamber is provided on the upper edge of the first lower opening, and a movable first lower adjustment plate is provided in the first lower accommodating chamber; a second lower opening is formed on the right side wall of the second groove, a second lower accommodating chamber is provided on the upper edge of the second lower opening, and a movable second lower adjustment plate is provided in the first lower accommodating chamber.

3. The device for detecting residual solvent in cigarette packaging materials according to claim 2, characterized in that: The first upper opening and the second upper opening have the same shape and size, and the first upper opening and the second upper opening are symmetrically arranged about a middle position of the first groove; The first lower opening and the second lower opening have the same shape and size, and the first lower opening and the second lower opening are symmetrically arranged about a middle position of the second groove.

4. The device for detecting residual solvent in cigarette packaging materials according to claim 2, characterized in that: The bottom surface of the first upper adjustment plate is provided with a first elastic layer, and the first elastic layer on the portion of the first upper adjustment plate extending from the first upper accommodating cavity abuts against the upper surface of the substrate; the bottom surface of the second upper adjustment plate is provided with a second elastic layer, and the second elastic layer on the portion of the second upper adjustment plate extending from the second upper accommodating cavity abuts against the upper surface of the substrate; A third elastic layer is arranged on the top surface of the first lower adjustment plate, and the third elastic layer on the portion of the first lower adjustment plate extending from the first lower accommodating cavity stops against the lower surface of the substrate; a fourth elastic layer is arranged on the top surface of the second lower adjustment plate, and the fourth elastic layer on the portion of the second lower adjustment plate extending from the second lower accommodating cavity stops against the lower surface of the substrate.

5. The device for detecting residual solvent in cigarette packaging materials according to claim 4, characterized in that: The first upper adjustment plate, the second upper adjustment plate, the first lower adjustment plate and the second lower adjustment plate are provided with scale lines.

6. The device for detecting residual solvent in cigarette packaging materials according to claim 1, characterized in that: The diameters of the first air inlet, the first air outlet, the second air inlet and the second air outlet are the same; the opening of the first groove is arranged opposite to the opening of the second groove, and the first groove and the second groove have the same shape and size; the first air inlet and the first air outlet are arranged symmetrically about the first groove; the second air inlet and the second air outlet are arranged symmetrically about the second groove.

7. A method for detecting residual solvents in cigarette packaging materials, characterized in that: include: introducing gas through the first air inlet and the second air inlet respectively; The gas introduced through the first gas inlet flows over the upper surface of the substrate, the solvent overflows from the upper surface of the substrate along with the gas, and the gas flows out from the first gas outlet; The gas introduced through the second gas inlet flows through the lower surface of the substrate, the solvent overflows from the lower surface of the substrate along with the gas, and the gas flows out from the second gas outlet; Respectively detecting the content and content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet; The source of the residual solvent in the packaging material is determined based on whether the content and the content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet are consistent.

8. The method for detecting residual solvents in cigarette packaging materials according to claim 7, characterized in that: The gas introduced into the first air inlet and the second air inlet includes an inert gas, and the solvent in the gas flowing out of the first air outlet and the second air outlet includes at least one of methanol, ethanol, propanol, benzene, toluene, xylene and acetone.

9. The method for detecting residual solvents in cigarette packaging materials according to claim 7, characterized in that: The determining of the source of the residual solvent in the packaging material according to whether the content and the content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet are consistent specifically includes: If the content and content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet of the substrate are consistent, the solvent in the substrate is residual during preparation; If at least one of the content and the content change rate of the solvent in the gas flowing out of the first gas outlet and the second gas outlet of the substrate is inconsistent, the solvent in the substrate is contaminated during storage and transportation.

10. The method for detecting residual solvents in cigarette packaging materials according to claim 7, characterized in that: The method for detecting residual solvents in the cigarette packaging material also includes: For the same batch of packaging material substrates, different areas are selected as sample substrates for testing. The source of the residual solvent in the packaging material is determined based on whether the content and content change rate of the solvent in the gas flowing through the upper and lower surfaces of the substrate in each area are consistent, including: If the solvent content and content change rate of the gas flowing out of the first gas outlet and the second gas outlet corresponding to each region of the substrate are consistent, the solvent in the substrate is residual during preparation; If at least one of the content and content change rate of the solvent in the gas flowing through the upper surface and the lower surface of the substrate in different areas is inconsistent, the solvent in the substrate is contaminated during storage and transportation.

Citation Information

Cited By

  • Testing device and testing method for residual solvent in cigarette packaging material

    WO2026061027A1