Cable for leakage sensor and preparation method

By designing leakage sensor cables with tinned copper conductors and polyphenylene sulfide wire braids, the problem of insufficient detection range and accuracy of existing sensors is solved, and wider detection and higher sensitivity are achieved, providing a focus on Remote monitoring and automatic early warning in the region improve the safety and reliability of the production environment.

CN118942769APending Publication Date: 2024-11-12LTK INDS HUIZHOU +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410987232.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing leak sensors have a small detection range and insufficient accuracy and sensitivity, which leads to difficult timely grasping the operating status of the pipeline network and failure to detect and deal with safety hazards in a timely manner. The detection technology is not reliable and cannot provide accurate safety risk warnings.

Method used

Design a cable for leakage sensors, including several twisted tinned copper conductors and an insulating layer braided on the outer periphery of the tinned copper conductor. The insulating layer is woven from polyphenylene sulfide wire and is placed on the insulating layer. The peripheral braided basalt yarn layer is used to identify leakage through the conductor resistance and conductivity changes of tin-plated copper conductors.

Benefits of technology

It improves the detection accuracy and sensitivity of leakage sensors, realizes remote monitoring and automatic early warning in key areas and high-risk areas, improves the timeliness and working quality of monitoring and early warnings, and provides a safer and more reliable production environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942769A_ABST
    Figure CN118942769A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of cables, in particular to a cable for a leakage sensor and a preparation method. A plurality of stranded tinned copper conductors and an insulating layer woven on the periphery of the tinned copper conductors are designed, the insulating layer is formed by weaving polyphenylene sulfide filaments, and a basalt yarn layer is woven on the periphery of the insulating layer. The tinned copper conductor is not easy to oxidize and has good appearance quality, and the polyphenylene sulfide wire has the advantages of high mechanical strength, high temperature resistance and chemical resistance. When liquid drops to the cable, the liquid permeates into the basalt yarn layer and the polyphenylene sulfide wire and can be in uniform contact with the tinned copper conductor, the purpose of leakage identification is achieved by influencing the conductor resistance and conductivity of the tinned copper conductor, and compared with an inductive probe, the detection range is wider, the accuracy and the sensitivity are improved, and the detection accuracy is improved. And a safer and more reliable production environment is brought to more industries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of cable technology, and in particular to a cable for a leakage sensor and a preparation method thereof. Background Art

[0002] At present, the construction of pipeline networks in industries such as new energy, semiconductors, oil depots, IDC data centers, petroleum, nonferrous metallurgy, and pharmaceuticals is facing a series of challenges. In the above industries, detection systems are often required to detect and alarm the leakage of various liquids such as water, oil, acid and alkali, and leakage sensors are usually used in current detection systems. In the industry, leakage sensors monitor a certain leakage source through a sensing probe, amplify, filter and condition the detected signal, and output the result to achieve the purpose of detection. However, the detection range of the sensing probe is small, and the accuracy and sensitivity need to be improved.

[0003] The above detection methods have the following two problems: 1. There is a large gap between the operation monitoring methods and safety needs, and effective operation monitoring methods have not kept up, resulting in difficulty in timely grasping the operation status of the pipeline network and safety hazards cannot be discovered and dealt with in a timely manner; 2. The current detection technology is not reliable and cannot provide accurate safety risk warnings. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a cable for a leakage sensor, comprising a plurality of twisted tinned copper conductors and an insulating layer woven around the periphery of the tinned copper conductors, wherein the insulating layer is woven with polyphenylene sulfide yarns, and a basalt yarn layer is woven around the periphery of the insulating layer.

[0005] Preferably, the polyphenylene sulfide yarn comprises the following raw material ratio: 100-110 parts of sodium sulfide nonahydrate, 90-100 parts of p-dichlorobenzene, 10-12 parts of dimethyl phosphamide, 7-10 parts of N-methyl caprolactam, 13-15 parts of aluminum chloride, 10-15 parts of sodium hydroxide, and 5-8 parts of basalt.

[0006] Preferably, the tin-copper conductor is composed of single crystal oxygen-free copper.

[0007] Preferably, there are seven tinned copper conductors, and the twisted structure is a co-core twisted structure with six outer conductors surrounding one central conductor.

[0008] Preferably, a preparation method for preparing the above-mentioned cable for leakage sensor comprises the following steps:

[0009] S1. preparing polyphenylene sulfide wire and tinned copper conductor;

[0010] S2, weaving the polyphenylene sulfide yarn on the outer periphery of the tinned copper conductor in an "8"-shaped curved track to form an insulating layer woven from polyphenylene sulfide;

[0011] S3. Weaving a basalt yarn layer around the outer periphery of the insulating layer.

[0012] Preferably, the preparation steps of the polyphenylene sulfide yarn are as follows:

[0013] A1. Add the above raw materials into a high-speed mixing pot, stir and heat to 150-160°C, and then extrude and granulate through a single screw extruder at 200°C to obtain uniform and transparent polyphenylene sulfide granules;

[0014] A2. Extruding the polyphenylene sulfide pellets through an extruder to form polyphenylene sulfide filaments.

[0015] Preferably, in step A2, the temperature of the screw section of the extruder is 280°C-360°C, and the temperature of the eye die section is 360°C.

[0016] Preferably, the tinned copper conductor (10) is a copper material consisting of a single grain drawn using a single crystal continuous casting technique.

[0017] As can be seen from the above, the following beneficial effects can be obtained by applying the present application: by designing a plurality of twisted tinned copper conductors and an insulating layer woven on the periphery of the tinned copper conductor, the insulating layer is woven with polyphenylene sulfide yarn, and a basalt yarn layer is woven on the periphery of the insulating layer. The tinned copper conductor is not easy to oxidize and has good appearance quality. The polyphenylene sulfide yarn has the advantages of high mechanical strength, high temperature resistance, and chemical resistance. When liquid drips onto the cable, the liquid penetrates into the basalt yarn layer and the polyphenylene sulfide yarn, and can evenly contact the tinned copper conductor, and achieve the purpose of leakage identification by affecting the conductor resistance and conductivity of the tinned copper conductor. Compared with the detection range of the induction probe, the detection accuracy and sensitivity of the leakage sensor are improved, and the key areas and key parts that may cause major accidents are targeted for key monitoring of medium and high risk areas and places, strengthen remote monitoring and automatic early warning, realize automatic alarm of abnormal safety conditions, improve the timeliness and work quality of monitoring and early warning, and bring a safer and more reliable production environment to more industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the description of the embodiments of the present application or the prior art are briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor.

[0019] Figure 1 This is a cable structure diagram for a leakage sensor according to an embodiment of the present application. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0021] Example

[0022] In order to solve the above technical problems, this embodiment provides a cable for a leakage sensor, such as Figure 1 As shown, it includes a plurality of twisted tinned copper conductors 10 and an insulating layer 20 woven on the periphery of the tinned copper conductor 10. The insulating layer 20 is woven with polyphenylene sulfide yarn, and a basalt yarn layer 30 is woven on the periphery of the insulating layer 20. The tinned copper conductor 10 is not easy to oxidize and has good appearance quality. The polyphenylene sulfide yarn has the advantages of high mechanical strength, high temperature resistance, and chemical resistance. When liquid drips onto the cable, the liquid penetrates into the basalt yarn layer 30 and the polyphenylene sulfide yarn, and can evenly contact the tinned copper conductor 10, and achieves leakage identification by affecting the conductor resistance and conductivity of the tinned copper conductor 10. Compared with the detection range of the induction probe, the cable of this scheme improves the detection accuracy and sensitivity of the leakage sensor, implements key monitoring for key areas, key parts and other medium and high risk areas and places that may cause major accidents, strengthens remote monitoring and automatic warning, realizes automatic alarm of abnormal safety conditions, and improves the timeliness and work quality of monitoring and warning, which will bring a safer and more reliable production environment to more industries.

[0023] Specifically, the polyphenylene sulfide yarn includes the following raw material ratios: 100-110 parts of sodium sulfide nonahydrate, 90-100 parts of p-dichlorobenzene, 10-12 parts of dimethyl ethyl phosphoramide, 7-10 parts of N-methyl caprolactam, 13-15 parts of aluminum chloride, 10-15 parts of sodium hydroxide, and 5-8 parts of basalt. Exemplarily, in the above raw material ratio, there are 108 parts of sodium sulfide nonahydrate, 100 parts of p-dichlorobenzene, 10 parts of dimethyl ethyl phosphoramide, 7 parts of N-methyl caprolactam, 13 parts of aluminum chloride, 10 parts of sodium hydroxide, and 5 parts of basalt.

[0024] The polyphenylene sulfide wire is woven around the outer periphery of the tinned copper conductor 10 in an "8"-shaped curved track. During weaving, the polyphenylene sulfide wire moves around the tinned copper conductor 10 in an "8"-shaped curved track in a circular and regular manner, and then weaves into an insulating layer 20, and then weaves the basalt yarn around the outer periphery of the insulating layer 20. Due to the characteristics of the weaving structure, when liquid drips onto the cable, the liquid penetrates into the basalt yarn layer 30 and the polyphenylene sulfide wire, and can evenly contact the tinned copper conductor 10, and then through the changes in the conductor resistance and conductivity of the tinned copper conductor 10, sensitive monitoring of liquid leakage and timely response to abnormal signals are achieved.

[0025] Furthermore, there are 7 tinned copper conductors 10, and the twisted structure is a co-core twisted structure with 6 outer conductors surrounding 1 central conductor. The surface of the tinned copper conductor 10 is tinned, not easy to oxidize and has a uniform appearance, and the contact between the tinned copper conductor 10 and the liquid can be sensitively monitored.

[0026] The basalt yarn layer 30 is woven with basalt yarn, which is an inorganic and environmentally friendly fiber material. It can be biodegraded in the environment after being discarded, is harmless to the environment, has high strength, and also has many excellent properties such as electrical insulation, corrosion resistance, and high temperature resistance. It has high strength, permanent flame retardancy, and short-term temperature resistance above 1000°C. It can be used for a long time in a temperature environment of 760°C. It can replace asbestos and glass fiber materials and has permanent flame retardancy. The cable using the structure of this application can meet the requirements that the resistance between the electrodes is greater than 100MΩ / 100m when the temperature is 24°C, the humidity is 60%RH, and the DC is 500V. Under high humidity and non-condensing conditions, the resistance between the electrodes exceeds 200KΩ / 100m when the temperature is 60°C and the humidity is 95%RH. The wire can operate continuously at a maximum temperature of 60°C. Cables using the structure of this application can achieve dynamic monitoring, implement key monitoring of medium and high risk areas and places such as key areas and key parts that may cause serious accidents, strengthen remote monitoring and automatic early warning, realize automatic alarm for abnormal safety situations, and improve the timeliness and work quality of monitoring and early warning.

[0027] This embodiment also provides a preparation method for preparing the above-mentioned cable for leakage sensor, comprising the following steps:

[0028] S1, preparing polyphenylene sulfide wire and tinned copper conductor 10;

[0029] In step S1, the tinned copper conductor 10 is a copper material composed of one crystal grain drawn out by single crystal continuous casting technology. This method enables the single crystal copper conductor to have a dense directional solidification structure, eliminates the transverse grain boundary, rarely has casting defects such as shrinkage holes and pores, and the crystallization direction is the same as the wire drawing direction, and can withstand greater plastic deformation capacity. The purity of ordinary oxygen-free copper is 99.95%, and the purity of this conductor can reach 99.9999%, with a minimum diameter specification of ф0.016mm, and the conductor resistance is 8%-13% lower than that of ordinary oxygen-free copper. Six co-core twisted tinned copper conductors are used around one in the middle. The conductor is not easy to oxidize and has a uniform appearance, and can be sensitively monitored when in contact with liquid. Automatic alarm for abnormal safety conditions is achieved, and the timeliness and work of monitoring and early warning are improved.

[0030] S2, weaving the polyphenylene sulfide yarn on the outer periphery of the tinned copper conductor 10 in an "8"-shaped curved track to form an insulating layer 20 woven from polyphenylene sulfide;

[0031] S3 . Weaving a basalt yarn layer 30 on the outer periphery of the insulating layer 20 .

[0032] In the above scheme, the preparation steps of polyphenylene sulfide silk are as follows:

[0033] A1. Take 108 parts of sodium sulfide nonahydrate, 100 parts of p-dichlorobenzene, 10 parts of dimethyl phosphamide, 7 parts of N-methyl caprolactam, 13 parts of aluminum chloride, 10 parts of sodium hydroxide, and 5 parts of basalt, add the above raw materials into a high-speed mixing pot, stir and heat to 150-160°C, and then extrude and granulate through a single screw extruder at 200-220°C to obtain uniform and transparent polyphenylene sulfide granules;

[0034] A2. Extruding the polyphenylene sulfide pellets through an extruder to form polyphenylene sulfide filaments.

[0035] Further, in step A2, the temperature of the screw section of the extruder is 280°C-360°C, and the temperature of the eye die section is 360°C.

[0036] The modified polyphenylene sulfide yarn obtained by the above raw material formula and process has outstanding thermal properties. The enhanced thermal performance indicators are as follows: maximum continuous use temperature 300°C: short-term maximum use temperature 420°C: heat deformation temperature 258°C, and has high mechanical strength, high temperature resistance, chemical resistance and other properties.

[0037] Furthermore, the polyphenylene sulfide wire is circulated and regularly moved in an "8"-shaped curved track around the tinned copper conductor 10, and then woven into an insulating layer 20, and then woven on the outer periphery of the insulating layer 20 by basalt yarn. Due to the characteristics of the woven structure, when liquid drips onto the wire, it can evenly contact the conductor, thereby achieving the transmission of the leakage signal by affecting the conductor resistance and conductivity of the conductor.

[0038] The cable prepared by the preparation method in this embodiment was tested and compared with the test results of the existing common sensor cables. Table 1 below is a comparison table of cable test results.

[0039]

[0040]

[0041] Table 1

[0042] It can be seen from Table 1 above that the modified polyphenylene sulfide yarn obtained by the above raw material formula and process, and the wire material designed by the above structure, have excellent thermal and mechanical properties. At the same time, after testing, when the temperature is 24°C, the humidity is 60% RH, and the DC is 500V, the resistance between the electrodes is greater than 100MΩ / 100m; when the temperature is 60°C, the humidity is 95% RH, and the DC is 500V, the resistance between the electrodes is greater than 200MΩ / 100m; and then a safe operation report can be generated online during operation, and a safety plan library, a knowledge base, etc. can be established according to the temperature and humidity of the environment and the resistance operation value between the two electrodes, to improve the auxiliary decision-making mechanism, provide scientific and effective predictability of emergency events, so that the wire can achieve emergency event auxiliary decision-making.

[0043] In summary, the present application scheme is achieved by designing a number of twisted tinned copper conductors and an insulating layer woven around the periphery of the tinned copper conductor. The insulating layer is woven with polyphenylene sulfide wire, and a basalt yarn layer is woven around the periphery of the insulating layer. The tinned copper conductor is not easily oxidized and has good appearance quality. The polyphenylene sulfide wire has the advantages of high mechanical strength, high temperature resistance, and chemical resistance. When liquid drips onto the cable, the liquid penetrates into the basalt yarn layer and the polyphenylene sulfide wire and can evenly contact the tinned copper conductor. The purpose of leakage identification is achieved by affecting the conductor resistance and conductivity of the tinned copper conductor. Compared with the detection range of the induction probe, the cable of this scheme improves the detection accuracy and sensitivity of the leakage sensor, which will bring a safer and more reliable production environment to more industries.

[0044] The above-described implementation methods do not constitute a limitation on the protection scope of the technical solution. Any modification, equivalent replacement and improvement made within the spirit and principle of the above-described implementation methods shall be included in the protection scope of the technical solution.

Claims

1. A cable for a leakage sensor, characterized in that: It comprises a plurality of twisted tinned copper conductors (10) and an insulating layer (20) woven around the periphery of the tinned copper conductor (10); the insulating layer (20) is woven with polyphenylene sulfide yarns, and a basalt yarn layer (30) is woven around the periphery of the insulating layer (20).

2. The cable for a leakage sensor according to claim 1, characterized in that: The polyphenylene sulfide yarn comprises the following raw material ratios: 100-110 parts of sodium sulfide nonahydrate, 90-100 parts of p-dichlorobenzene, 10-12 parts of dimethyl ethylphosphamide, 7-10 parts of N-methyl caprolactam, 13-15 parts of aluminum chloride, 10-15 parts of sodium hydroxide and 5-8 parts of basalt.

3. The cable for a leakage sensor according to claim 1, characterized in that: The tin-copper conductor (10) is composed of single-crystal oxygen-free copper.

4. The cable for a leakage sensor according to claim 3, characterized in that: There are seven tinned copper conductors (10), and the twisted structure is a co-core twisted structure in which six outer conductors are twisted around one central conductor.

5. A preparation method, characterized in that: The method for preparing the cable for the leakage sensor according to any one of claims 2 to 4 comprises the following steps: S1, preparing polyphenylene sulfide filaments and tinned copper conductors (10); S2, weaving the polyphenylene sulfide yarn on the outer periphery of the tinned copper conductor (10) in an "8"-shaped curved track to form an insulating layer (20) woven from polyphenylene sulfide; S3. Weaving a basalt yarn layer (30) around the outer periphery of the insulating layer (20).

6. The preparation method according to claim 5, characterized in that: The preparation steps of the polyphenylene sulfide silk are as follows: A1. Add the above raw materials into a high-speed mixing pot, stir and heat to 150-160°C, and then extrude and granulate through a single screw extruder at 200-220°C to obtain uniform and transparent polyphenylene sulfide granules; A2. Extruding the polyphenylene sulfide pellets through an extruder to form polyphenylene sulfide filaments.

7. The preparation method according to claim 6, characterized in that: In step A2, the temperature of the screw section of the extruder is 280°C-360°C, and the temperature of the eye die section is 360°C.

8. The preparation method according to claim 5, characterized in that: The tinned copper conductor (10) is a copper material consisting of a single crystal grain drawn out by single crystal continuous casting technology.