Nanocrystalline copper-silver alloy current collector and preparation method thereof
By preparing nanocrystalline copper-silver alloy current collectors and controlling the silver content using direct current electrodeposition, the problem of uneven lithium nucleation caused by the uneven surface of copper foil current collectors was solved, achieving uniform lithium deposition, inhibiting lithium dendrite growth, and improving the strength and conductivity of the current collectors.
Patent Information
- Application Number
- CN202411246944.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The uneven surface of existing copper foil current collectors leads to uneven nucleation of metallic lithium, which easily forms lithium dendrites. Furthermore, existing alloy layer modification methods result in a loss of conductivity and insufficient interfacial bonding.
Nanocrystalline copper-silver alloy current collectors were prepared by direct current electrodeposition. Silver element dispersed lithium nucleation sites and reduced the nucleation barrier. By controlling the deposition current density and plating solution composition, the silver content was kept between 1% and 15%, thus achieving uniform lithium deposition.
It effectively inhibits lithium dendrite growth, improves current collector strength and conductivity, and enhances the stability and safety of lithium metal anodes.
Smart Images

Figure BDA0005031050900000051 
Figure BDA0005031050900000061 
Figure HDA0005031050920000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of batteries, and in particular to a nanocrystalline copper-silver alloy current collector and a preparation method thereof. Background Art
[0002] With the rapid rise of industries such as mobile phones, smart watches, and electric vehicles, the market demand for energy storage batteries with high energy density and high safety is becoming increasingly urgent. Among many battery technologies, metallic lithium has become the focus of research on the next generation of battery negative electrode materials due to its impressive theoretical specific energy (up to 3860mAh / g) and extremely low redox electrode potential (-3.040V standard hydrogen electrode). However, metallic lithium negative electrodes are prone to form needle-shaped or tree-shaped lithium dendrites during the charge and discharge cycle, which not only leads to irreversible loss of battery capacity, but may also cause internal short circuits in the battery due to piercing the diaphragm, thereby bringing safety risks such as overheating and spontaneous combustion. In order to solve these problems, scientific researchers have made many attempts from the perspectives of material structure design and battery structure design, but at present, they cannot perfectly solve the problems of low cycle efficiency, poor stability, and low safety of metallic lithium negative electrodes. New perspectives and new strategies are needed to inhibit the growth of lithium dendrites.
[0003] The initial nucleation and growth stage of metallic lithium has a crucial influence on its subsequent deposition process, which directly determines the stability of the subsequent metallic lithium. Therefore, effectively controlling the nucleation and growth of metallic lithium, especially ensuring the uniform nucleation of metallic lithium, has become the key to inhibiting the growth of lithium dendrites. However, the copper foil current collector currently widely used is prone to uneven enrichment during the nucleation stage of metallic lithium due to its uneven surface and existing defects, which greatly increases the risk of lithium dendrites. Therefore, seeking a negative electrode current collector that can induce uniform nucleation of lithium metal is particularly important for the development of lithium metal negative electrodes.
[0004] At present, the negative electrode current collector method that induces uniform nucleation of lithium metal often forms an alloy layer on the surface of the existing copper current collector by introducing alloy elements to modify the surface of the existing copper current collector. On the one hand, this modification method will sacrifice the conductive properties of the original current collector, and on the other hand, there will be problems with poor interface bonding. For example: Patent CN108550858A discloses a copper-zinc alloy current collector that inhibits lithium dendrites. In this patent, a layer of copper-tin alloy is coated on the base material by magnetron sputtering. Patent CN114400331A discloses a method for preparing a negative electrode current collector that can improve the cycle stability of metallic lithium. In this patent, a layer of copper-tin alloy is coated on the surface of copper foil by physical vapor deposition.
[0005] The above methods all simply cover the copper foil surface with an alloy layer, which greatly sacrifices the original current collector conductivity to improve the growth of lithium dendrites, and there are also problems such as poor interface bonding. Therefore, it is necessary to find a new method that can induce uniform nucleation of lithium metal without serious loss of conductivity and excellent interface bonding. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. In order to inhibit the growth of lithium dendrites, improve the stability and safety of lithium metal negative electrodes, and increase the strength of current collectors without seriously losing conductivity, the present invention provides a nanocrystalline copper-silver alloy current collector and a preparation method thereof. The silver element in the copper-silver alloy current collector can disperse the nucleation sites of metallic lithium, reduce the nucleation barrier, and induce uniform deposition of metallic lithium. The nanocrystalline copper-silver alloy current collector in the present invention is realized by a direct current deposition method. In the present invention, nanocrystalline copper-silver alloy foil replaces copper foil as the negative electrode current collector, wherein the content of silver atoms in the copper-silver alloy is 1% to 15%, which is achieved by controlling the deposition current density or the composition of the plating solution.
[0007] In the first aspect of the present invention, the present invention proposes a nanocrystalline copper-silver alloy current collector. According to an embodiment of the present invention, the content of silver atoms in the nanocrystalline copper-silver alloy current collector is 1% to 15%. The silver element in the copper-silver alloy current collector can disperse the nucleation sites of metallic lithium, reduce the nucleation barrier, and induce uniform deposition of metallic lithium.
[0008] In another aspect of the present invention, the present invention also proposes a method for preparing a nanocrystalline copper-silver alloy current collector. According to an embodiment of the present invention, the method comprises:
[0009] 1) copper sulfate, potassium pyrophosphate and deionized water are mixed to obtain a mixed solution A;
[0010] 2) Mix potassium iodide, potassium nitrate, silver nitrate and deionized water to obtain a mixed solution B;
[0011] 3) mixing the solution A with the solution B to obtain a solution C;
[0012] 4) mixing the refiner with the C solution to obtain a D solution,
[0013] 5) Placing the anode copper plate and the cathode nickel plate into the D solution for deposition treatment to obtain the nanocrystalline copper-silver alloy current collector. By controlling the deposition current density or the composition of the plating solution, the content of silver atoms in the copper-silver alloy can be 1% to 15%. The silver element in the copper-silver alloy current collector can disperse the nucleation sites of metallic lithium, reduce the nucleation barrier, and induce uniform deposition of metallic lithium.
[0014] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:
[0015] According to an embodiment of the present invention, in step 1), the mass concentration ratio of the copper sulfate to the potassium pyrophosphate is (20-100): (60-300).
[0016] According to an embodiment of the present invention, in step 1), the mass concentration ratio of the copper sulfate to the potassium pyrophosphate is (50-80):(150-240).
[0017] According to an embodiment of the present invention, in step 2), the mass concentration ratio of the potassium iodide, the potassium nitrate and the silver nitrate is (150-240):(5-15):(0.15-1.5).
[0018] According to an embodiment of the present invention, in step 2), the usage ratio of the A solution to the B solution is 1:1.2.
[0019] According to an embodiment of the present invention, in step 2), the dosage ratio of the A solution to the B solution is 1:1.
[0020] According to an embodiment of the present invention, the temperature of the mixing process is 40-60°C.
[0021] According to an embodiment of the present invention, the mixing process is performed under stirring, and the stirring speed is 200-800 rpm.
[0022] According to an embodiment of the present invention, the thinning agent is thiourea, 2-mercaptobenzimidazole or sodium polydisulfide dipropane sulfonate.
[0023] According to an embodiment of the present invention, the deposition process is performed using a direct current power source.
[0024] According to an embodiment of the present invention, the current density of the DC power supply is 2-20 mA / cm 2 .
[0025] According to an embodiment of the present invention, the deposition process takes 30 to 120 minutes.
[0026] According to an embodiment of the present invention, the anode copper plate and the cathode nickel plate are anode copper plates and cathode nickel plates that have been polished, washed with water, cleaned with anhydrous ethanol, and then dried.
[0027] In another aspect of the present invention, the present invention further provides a battery. According to an embodiment of the present invention, the battery comprises the nanocrystalline copper-silver alloy current collector described above or the nanocrystalline copper-silver alloy current collector prepared according to the method described above. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0029] Figure 1 is a SEM image of lithium deposited on a nanocrystalline copper-silver alloy current collector according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0031] Example 1
[0032] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0033] 2. Prepare mixed solution B according to the following component proportions: weigh 150 g / L potassium iodide, 10 g / L potassium nitrate, and 0.34 g / L silver nitrate;
[0034] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0035] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0036] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 5 mA / cm2, the deposition time is 60 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0037] Example 2
[0038] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0039] 2. Prepare mixed solution B according to the following component proportions: potassium iodide 150g / L, potassium nitrate 10g / L, silver nitrate 0.68g / L;
[0040] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0041] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0042] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 5 mA / cm2, the deposition time is 60 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0043] Example 3
[0044] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0045] 2. Prepare mixed solution B according to the following component proportions: potassium iodide 150g / L, potassium nitrate 10g / L, silver nitrate 1.02g / L;
[0046] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0047] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0048] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 5 mA / cm2, the deposition time is 60 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0049] Example 4
[0050] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0051] 2. Prepare mixed solution B according to the following component proportions: potassium iodide 150g / L, potassium nitrate 10g / L, silver nitrate 1.36g / L;
[0052] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0053] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0054] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 10 mA / cm2, the deposition time is 60 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0055] Example 5
[0056] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0057] 2. Prepare mixed solution B according to the following component proportions: potassium iodide 150g / L, potassium nitrate 10g / L, silver nitrate 0.34g / L;
[0058] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0059] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0060] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 10 mA / cm2, the deposition time is 30 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0061] Example 6
[0062] 1. Prepare mixed solution A according to the following component proportions: copper sulfate 50g / L, potassium pyrophosphate 150g / L;
[0063] 2. Prepare mixed solution B according to the following component proportions: potassium iodide 150g / L, potassium nitrate 10g / L, silver nitrate 0.34g / L;
[0064] 3. Mix solution A obtained in step 1 with solution B obtained in step 2 to obtain solution C;
[0065] 4. Dissolve 0.005 g / L thiourea in the solution C obtained in step 3 according to the above component ratio to obtain solution D;
[0066] 5. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode nickel plate into the D solution obtained in step 4, use a DC power supply for deposition, the current density is 15 mA / cm2, the deposition time is 20 min, the constant temperature is 50 ° C, the stirring speed is 200 rpm, and the nanocrystalline copper-silver alloy current collector is peeled off from the substrate.
[0067] Comparative Example 1
[0068] 1. Prepare mixed solution A according to the following component proportions: 120 g / L copper sulfate, 100 g / L copper chloride, and 60 g / L concentrated sulfuric acid;
[0069] 2. Add 0.02 g / L sodium polydisulfide dipropane sulfonate and 0.01 g / L sodium dodecylbenzene sulfonate in equal proportions to the solution A obtained in step 1 to obtain a solution B;
[0070] 3. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode stainless steel plate into solution B obtained in step 2, use a DC power supply for deposition, the current density is 10 mA / cm2, the deposition time is 30 min, the constant temperature is 25 ° C, the stirring speed is 500 rpm, and the copper foil current collector is peeled off from the substrate.
[0071] Comparative Example 2
[0072] 1. Prepare mixed solution A according to the following component proportions: 120 g / L copper sulfate, 100 g / L copper chloride, and 60 g / L concentrated sulfuric acid;
[0073] 2. Add 0.02 g / L sodium thiosulfonate, 0.01 g / L ethylenethiourea, and 0.01 g / L polyethylene glycol in equal proportions to the solution A obtained in step 1 to obtain a solution B;
[0074] 3. Place the polished, washed, cleaned with anhydrous ethanol and dried anode copper plate and cathode stainless steel plate into solution B obtained in step 2, use a DC power supply for deposition, the current density is 10 mA / cm2, the deposition time is 30 min, the constant temperature is 25 ° C, the stirring speed is 500 rpm, and the copper foil current collector is peeled off from the substrate.
[0075] It can be seen from the data in the table below that the nanocrystalline copper-silver alloy current collector obtained by the embodiment of the present invention has higher strength and good electrical conductivity. Figure 1 It can be seen that lithium metal is deposited on the surface of the nanocrystalline copper-silver alloy current collector obtained by the embodiment of the present invention, and it is found that it can induce uniform nucleation of lithium metal and effectively prevent the formation of lithium dendrites, thereby improving the cycle stability of the lithium metal negative electrode.
[0076] Table 1 Silver content, current collector strength and conductivity of the embodiments and comparative examples
[0077]
[0078]
[0079] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0080] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A nanocrystalline copper-silver alloy current collector, characterized in that: The content of silver atoms in the nanocrystalline copper-silver alloy current collector is 1% to 15%.
2. A method for preparing a nanocrystalline copper-silver alloy current collector, characterized in that: include: 1) copper sulfate, potassium pyrophosphate and deionized water are mixed to obtain solution A; 2) Mix potassium iodide, potassium nitrate, silver nitrate and deionized water to obtain solution B; 3) mixing the solution A with the solution B to obtain a solution C; 4) mixing the refiner with the C solution to obtain a D solution, 5) placing the anode copper plate and the cathode nickel plate into the D solution for deposition treatment to obtain the nanocrystalline copper-silver alloy current collector.
3. The method according to claim 2, characterized in that The mass concentration ratio of the copper sulfate and the potassium pyrophosphate in step 1) is (20-100): (60-300); Preferably, in step 1), the mass concentration ratio of the copper sulfate to the potassium pyrophosphate is (50-80):(150-240).
4. The method according to claim 2, characterized in that: In step 2), the mass concentration ratio of the potassium iodide, the potassium nitrate and the silver nitrate is (150-240):(5-15):(0.15-1.5).
5. The method according to claim 2, characterized in that: In step 2), the dosage ratio of solution A to solution B is 1:1.2; Optionally, in step 2), the dosage ratio of the A solution to the B solution is 1:
1.
6. The method according to claim 2, wherein the temperature of the mixing treatment is 40 to 60°C; Optionally, the mixing process is performed under stirring, and the stirring speed is 200-800 rpm.
7. The method according to claim 2, wherein the thinning agent is thiourea, 2-mercaptobenzimidazole or sodium polydisulfide dipropane sulfonate.
8. The method according to claim 2, wherein the deposition process is performed using a direct current power supply; Optionally, the current density of the DC power supply is 2-20 mA / cm 2 ; Optionally, the deposition treatment time is 30 to 120 minutes.
9. The method according to claim 2, wherein the anode copper plate and the cathode nickel plate are polished, washed, cleaned with anhydrous ethanol and then dried.
10. A battery, characterized in that: The battery comprises the nanocrystalline copper-silver alloy current collector according to claim 1 or the nanocrystalline copper-silver alloy current collector prepared by the method according to any one of claims 2-9.
Citation Information
Patent Citations
Cyanide-free zinc dipping solution and cyanide-free electroplating method of filter aluminium alloy by using the same
CN102732922A
Preparation method of three-dimensional current collecting structure for lithium battery electrode material
CN104752732A
Three-dimensional metal-based lithium-loving current collector, lithium metal negative electrode and lithium metal battery
CN115881973A
Method for preparing nanoscale dendritic crystal copper powder through electro-deposition
CN117210876A
Copper or copper-alloy foil for circuit
JP2007107037A
Cited By
Heterogeneous copper alloy current collector and preparation method and application thereof
CN119812353A
A heterogeneous copper alloy current collector, its preparation method and application
CN119812353B