Gel electrolyte precursor, gel electrolyte, preparation method of gel electrolyte precursor and preparation method of gel electrolyte, and battery
By using gel electrolyte precursor and dispersion medium with specific structures in the battery cell for polymerization reaction, semi-solid gel electrolyte is formed, which solves the problem of insufficient safety of overcharge of traditional gel electrolytes in the battery cell and improves the battery cell The effect of security.
Patent Information
- Application Number
- CN202310528467.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional gel electrolytes have shortcomings in battery cell overcharge safety, resulting in insufficient safety of power batteries, especially the application of high-energy-density power batteries.
Using a gel electrolyte precursor, including compounds of specific structures, plasticizers and lithium salts, polymerization reactions in the presence of a dispersion medium to form a semi-solid gel electrolyte, reducing the amount of electrolyte and passing electrochemistry when overcharged Polymerization forms polymer penetrates the membrane, consumes charging power, and improves the overcharge safety of the battery cell.
It effectively improves the safety of the battery cell, and improves the safety performance of the overall battery cell by reducing the amount of electrolyte and forming a micro-short circuit during overcharge.
Smart Images

Figure BDA0004223770350000021 
Figure BDA0004223770350000022 
Figure BDA0004223770350000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of power batteries, and in particular to a gel electrolyte precursor, a gel electrolyte, a preparation method thereof, and a battery. Background Art
[0002] With the general trend of carbon peak and carbon neutrality, electric vehicles have increasingly replaced traditional fuel vehicles and become an important means of transportation for people, which has also driven the development and application of power batteries. With the development and iteration of power batteries, high-energy-density batteries have gradually become the mainstream of the market. However, the safety of high-energy-density power batteries is still an important issue restricting their development. Vehicle fires and explosions caused by battery safety issues have, to a certain extent, restricted the application of power batteries, especially high-energy-density power batteries.
[0003] Gel electrolyte is an electrolyte in a gel state, which can replace part of the electrolyte inside the battery cell, reducing the amount of electrolyte used and thus improving the safety of the battery cell. However, traditional gel electrolytes still have shortcomings in improving the overcharge safety of the battery cell. Summary of the invention
[0004] Based on this, the present invention provides a gel electrolyte precursor, a gel electrolyte and a preparation method thereof and a battery to solve the problem that traditional gel electrolytes have shortcomings in terms of battery cell overcharge safety.
[0005] The first aspect of the present invention provides a gel electrolyte precursor, and its technical solution is as follows:
[0006] A gel electrolyte precursor, comprising a compound having a structure shown in formula I, a plasticizer and a lithium salt;
[0007]
[0008] Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
[0009] In some embodiments, the compound with the structure shown in Formula I accounts for 20% to 60% by mass in the gel electrolyte precursor.
[0010] In some embodiments, the plasticizer accounts for 20% to 60% by weight in the gel electrolyte precursor.
[0011] In some of the embodiments, the plasticizer is selected from at least one of succinonitrile, trans-butenedinitrile, adiponitrile, glutaronitrile, suberonitrile and sebaconitrile.
[0012] In some embodiments, the lithium salt accounts for 1% to 20% by mass in the gel electrolyte precursor.
[0013] In some embodiments, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorooxalatoborate and lithium tetrafluoroborate.
[0014] In some embodiments, the lithium salt further comprises at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium bis(oxalate borate) and the like.
[0015] The second aspect of the present invention provides a gel electrolyte, and its technical solution is as follows:
[0016] A gel electrolyte comprising a compound of the structure shown in Formula II, a plasticizer, a lithium salt and a dispersion medium;
[0017]
[0018] Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
[0019] In some embodiments, the dispersion medium includes an electrolyte.
[0020] In some of the embodiments, the mass ratio of the gel electrolyte precursor to the electrolyte is (1-7):(9-3).
[0021] In some embodiments, the solvent of the electrolyte is selected from at least one of dimethyl carbonate and ethyl methyl carbonate.
[0022] In some embodiments, the solvent of the electrolyte is a mixture of dimethyl carbonate and ethyl methyl carbonate, wherein the volume ratio of dimethyl carbonate to ethyl methyl carbonate is 1:(1-3).
[0023] The third aspect of the present invention provides a method for preparing a gel electrolyte, and the technical scheme thereof is as follows:
[0024] The above-mentioned gel electrolyte precursor is subjected to a polymerization reaction in the presence of a dispersion medium.
[0025] The fourth aspect of the present invention also provides a battery, and its technical solution is as follows:
[0026] A battery comprises the above-mentioned gel electrolyte.
[0027] In some of the embodiments, a positive electrode plate is further included, and the gel electrolyte is located on the positive electrode plate.
[0028] Compared with the traditional solution, the present invention has the following beneficial effects:
[0029] The present invention uses a compound with a structure shown in Formula I as a gel skeleton monomer. On the one hand, the compound with a structure shown in Formula I can undergo an epoxy polymerization reaction in the presence of a plasticizer, a lithium salt and a dispersion medium to form a semi-solid gel electrolyte, replace a portion of the electrolyte, reduce the amount of electrolyte used, and thus improve the safety of the battery cell; on the other hand, when the battery is overcharged, the 2-biphenyl group in the compound with a structure shown in Formula I will further undergo electrochemical polymerization, and the formed polymer can penetrate the diaphragm to cause a micro-short circuit in the battery cell, consume charging energy, and can improve the overcharge safety of the battery cell, so as to achieve the purpose of improving the safety of the overall battery cell. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0032] the term
[0033] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0034] In the present invention, the selection range involving "and / or", "or / and", and "and / or" includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the arbitrary and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution that is all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four of A, B, C, and D (that is, the technical solution that is all connected by "logical AND").
[0035] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0036] In the present invention, "combinations thereof", "any combinations thereof", "any combination thereof" and the like include all suitable combinations of any two or more of the listed items.
[0037] In the present invention, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the ability to implement the technical solution of the present invention, solve the technical problem of the present invention, and achieve the expected technical effect of the present invention.
[0038] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0039] In the present invention, the words “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0040] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0041] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0042] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0043] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0044] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0045] In the present invention, when it comes to percentage content, unless otherwise specified, for solid-liquid mixing and solid-solid mixing, it refers to mass percentage, and for liquid-liquid mixing, it refers to volume percentage.
[0046] In the present invention, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0047] In the present invention, % (w / w) and wt% both represent weight percentage, % (v / v) refers to volume percentage, and % (w / v) refers to mass volume percentage.
[0048] In the present invention, room temperature refers to a temperature of 10°C to 30°C.
[0049] In view of the problem that traditional gel electrolytes still have shortcomings in terms of overcharge safety of battery cells, the present invention provides a gel electrolyte precursor. In one embodiment, the gel electrolyte precursor includes a compound with a structure shown in Formula I, a plasticizer and a lithium salt;
[0050]
[0051] Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
[0052] In this embodiment, the compound of the structure shown in Formula I is used as a gel skeleton monomer. On the one hand, the compound of the structure shown in Formula I can undergo a polymerization reaction in the presence of a plasticizer, a lithium salt, a lithium salt and a dispersion medium to form a semi-solid gel electrolyte, replace a portion of the electrolyte, reduce the amount of electrolyte, and thus improve the safety of the battery cell; on the other hand, when the battery is overcharged, the 2-biphenyl in the compound of the structure shown in Formula I will further undergo electrochemical polymerization, and the formed polymer can penetrate the diaphragm to cause a micro-short circuit in the battery cell, consume charging energy, and thus improve the overcharge safety of the battery cell, so as to achieve the purpose of improving the safety of the overall battery cell.
[0053] At present, commercialized gel electrolytes mainly include polyacrylonitrile (PAN)-based polymerization systems, polyvinylidene fluoride (PVDF)-based polymerization systems, and polymethyl methacrylate (PMMA)-based polymerization systems. Different from the above-mentioned polymerization systems, the gel electrolyte precursor of this embodiment can form a gel electrolyte with a new polymerization system.
[0054] Optionally, the mass proportion of the compound of the structure shown in Formula I in the gel electrolyte precursor is 20% to 60%. For example, the mass proportion of the compound of the structure shown in Formula I in the gel electrolyte precursor includes but is not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%.
[0055] Optionally, when R1 and R2 are both H, the compound with the structure shown in Formula I is 2-biphenyl glycidyl ether.
[0056] In this embodiment, the plasticizer is beneficial to increase the conductivity of lithium ions.
[0057] Optionally, the mass proportion of the plasticizer in the gel electrolyte precursor is 20% to 60%. For example, the mass proportion of the plasticizer in the gel electrolyte precursor includes but is not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%.
[0058] Optionally, the plasticizer is selected from at least one of succinonitrile, trans-butenedinitrile, adiponitrile, glutaronitrile, suberonitrile and sebaconitrile.
[0059] Optionally, the mass proportion of the lithium salt in the gel electrolyte precursor is 1% to 20%. For example, the mass proportion of the lithium salt in the gel electrolyte precursor includes but is not limited to 1%, 2%, 3%, 4%, 5%, 8%, 10%, 12%, 15%, 18%, 20%.
[0060] Optionally, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorooxalatoborate (LiDFOB) and lithium tetrafluoroborate (LiBF4).
[0061] Further optionally, the lithium salt also includes at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalate borate), and .
[0062] The present invention also provides a gel electrolyte. In one embodiment, the gel electrolyte includes a compound of the structure shown in Formula II, a plasticizer, a lithium salt and a dispersion medium;
[0063]
[0064] Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
[0065] The plasticizer and lithium salt are as described above and will not be described in detail here.
[0066] Optionally, the dispersion medium includes an electrolyte.
[0067] Optionally, the mass ratio of the gel electrolyte precursor to the electrolyte is (1-7):(9-3).
[0068] Optionally, the electrolyte may be a commonly used basic electrolyte, for example, the electrolyte comprises the following components in percentage by mass: 15-28% lithium salt, 1-10% additive, and 70-84% solvent.
[0069] Optionally, the lithium salt in the electrolyte is selected from at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium bis(oxalyl)borate and lithium tetrafluoroborate.
[0070] Optionally, the additive in the electrolyte is selected from at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC) and chloroethylene carbonate (CEC).
[0071] Optionally, the solvent of the electrolyte does not contain ethylene carbonate (EC).
[0072] Optionally, the solvent of the electrolyte is selected from at least one of dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC).
[0073] Optionally, the solvent of the electrolyte is a mixture of DMC and EMC, wherein the volume ratio of DMC to EMC is 1:(1-3). For example, the volume ratio of DMC to EMC is 1:1, 1:2, or 1:3.
[0074] The gel electrolyte of this embodiment is resistant to high voltage and can be applied to automotive power batteries, for example, power batteries of a high nickel system.
[0075] The present invention also provides a method for preparing a gel electrolyte. In one embodiment, the method for preparing a gel electrolyte comprises the following steps:
[0076] The above-mentioned gel electrolyte precursor is subjected to a polymerization reaction in the presence of a dispersion medium.
[0077] In this embodiment, the gel electrolyte precursor undergoes a polymerization reaction in the presence of a dispersion medium to improve the use effect of the gel electrolyte.
[0078] Optionally, the polymerization reaction can be carried out at room temperature, for example, slowly polymerizing at room temperature to form a semi-solid gel electrolyte. The gel electrolyte precursor can also be solidified into a semi-solid gel electrolyte under other conditions. For example, the polymerization reaction can be a thermal polymerization reaction or an electropolymerization reaction.
[0079] When the polymerization reaction is a thermal polymerization reaction, the polymerization temperature may be 60° C. to 100° C. The polymerization time may be 20 h to 28 h.
[0080] When the dispersion medium includes an electrolyte, the gel electrolyte precursor is mixed with the electrolyte and then subjected to polymerization reaction to form a semi-solid gel electrolyte.
[0081] It can be understood that when the gel electrolyte precursor and the electrolyte are mixed, the temperature can be room temperature and the humidity can be a dew point of ≤-40°C.
[0082] The electrolyte is as described above and will not be described in detail here.
[0083] The present invention also provides a battery. In one embodiment, the battery comprises the above-mentioned gel electrolyte.
[0084] Optionally, the battery further comprises a positive electrode plate, and the gel electrolyte is located on the positive electrode plate.
[0085] In the battery of this embodiment, the gel electrolyte is located on the positive electrode plate. Since the positive electrode plate and the negative electrode plate are separated by a diaphragm, the adverse effects of the biphenyl compounds contained in the gel electrolyte on the negative electrode plate, such as affecting the film formation of the negative electrode and causing a decrease in battery performance, can be avoided. At the same time, the 2-biphenyl in the gel electrolyte can further undergo electrochemical polymerization on the positive electrode plate side when overcharged, increasing the impedance of the positive electrode plate side of the battery cell and improving the overcharge safety performance of the battery cell.
[0086] Optionally, the gel electrolyte may be formed on the positive electrode plate side by in-situ polymerization. It can be understood that the gel electrolyte is located on the corresponding two sides of the positive electrode plate.
[0087] Optionally, the method for forming a gel electrolyte on the positive electrode plate comprises the following steps:
[0088] The gel electrolyte precursor is mixed with a dispersion medium to obtain a mixed solution, and the mixed solution is brought into contact with a positive electrode plate, and then a gel electrolyte is formed on the positive electrode plate through a polymerization reaction.
[0089] It can be understood that, through the above contact, the internal pores of the positive electrode sheet can absorb the gel electrolyte precursor. Before the polymerization reaction, the positive electrode sheet that absorbs the gel electrolyte precursor is also dried.
[0090] Optionally, the mixed solution may contact the positive electrode plate by referring to the following two methods:
[0091] Method 1: Spray the mixed liquid onto the positive electrode.
[0092] Method 2: Immerse the positive electrode into the mixed solution and take it out.
[0093] Understandably, considering the involvement of other work sections and equipment installation, a suitable method can be selected based on the close integration of the polymerization process and the battery cell production process in large-scale production.
[0094] The positive electrode plate with gel electrolyte can be sealed in an inert gas (N2) storage cabinet for future use.
[0095] In this embodiment, the positive electrode sheet with gel electrolyte, the separator and the negative electrode sheet are stacked to form a cell, and then a battery is assembled.
[0096] In this embodiment, the battery is a semi-solid-state battery.
[0097] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0098] Example 1
[0099] This embodiment provides a battery cell and a method for preparing the same, the steps are as follows:
[0100] Step 1: Preparation of gel electrolyte precursor
[0101] The components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0102] 2-Biphenyl glycidyl ether 42%, succinonitrile 42%, lithium hexafluorophosphate 1%, lithium bis(trifluoromethanesulfonyl)imide 15%.
[0103] Step 2: Prepare a mixture of a gel electrolyte precursor and an electrolyte
[0104] At room temperature and a dew point humidity of ≤-40° C., the gel electrolyte precursor and the electrolyte are mixed in a volume ratio of 4:6, and stirred evenly to obtain a mixed solution.
[0105] The electrolyte is composed of the following components in percentage by mass: 18% lithium bis(trifluoromethanesulfonyl)imide, 2% vinylene carbonate, and 80% solvent, wherein the solvent is a mixture of DMC:EMC in a volume ratio of 1:1.
[0106] Step 3: Forming a gel electrolyte on the positive electrode
[0107] At room temperature and a dew point humidity of ≤-40°C, the mixed solution is uniformly sprayed on the positive electrode plate. After drying, in-situ polymerization is carried out at 80°C and a dew point humidity of ≤-40°C for 24 hours to obtain a positive electrode plate with a gel electrolyte.
[0108] Step 4: Prepare the battery cell
[0109] The positive electrode sheet with gel electrolyte, the separator and the negative electrode sheet stack are assembled into a battery cell.
[0110] Example 2
[0111] This embodiment provides a battery cell and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the gel electrolyte precursor is different. In this embodiment, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0112] 2-Biphenyl glycidyl ether 50%, succinonitrile 34%, lithium hexafluorophosphate 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0113] Example 3
[0114] This embodiment provides a battery cell and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the gel electrolyte precursor is different. In this embodiment, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0115] 2-Biphenyl glycidyl ether 55%, succinonitrile 29%, LiDFOB 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0116] Example 4
[0117] This embodiment provides a battery cell and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the gel electrolyte precursor is different. In this embodiment, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0118] 2-Biphenyl glycidyl ether 60%, succinonitrile 24%, LiBF4 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0119] Example 5
[0120] This embodiment provides a battery cell and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the gel electrolyte precursor is different. In this embodiment, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0121] 2-Biphenyl glycidyl ether 35%, adiponitrile 49%, LiDFOB 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0122] Example 6
[0123] This embodiment provides a battery cell and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the gel electrolyte precursor is different. In this embodiment, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0124] 2-Biphenyl glycidyl ether 30%, adiponitrile 54%, LiDFOB 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0125] Comparative Example 1
[0126] This comparative example provides a battery cell and a preparation method thereof, the steps are as follows:
[0127] Referring to Example 1, the positive electrode sheet, the separator and the negative electrode sheet are directly assembled into a battery cell.
[0128] Comparative Example 2
[0129] This comparative example provides a battery cell and a preparation method thereof, which is basically the same as Example 3, except that the gel electrolyte precursor is different. In this example, the components are mixed according to the following mass percentages to obtain a gel electrolyte precursor:
[0130] Triglycidyl ether 55%, succinonitrile 29%, LiDFOB 5%, lithium bis(trifluoromethanesulfonyl)imide 11%.
[0131] The cells of each embodiment and comparative example were evaluated according to the following evaluation method:
[0132] Standard capacity:
[0133] 1-1) 25±2℃, let stand for 5min;
[0134] 1-2) 25±2℃, charge to 4.25V with 1 / 3C CC-CV, and the cut-off current is 1 / 20C;
[0135] 1-3) 25±2℃, let stand for 30min;
[0136] 1-4) 25±2℃, discharge to 2.5V at 1 / 3C;
[0137] 1-5) 25±2℃, stand for 30min;
[0138] 1-6) Repeat steps 1-2) to 1-5); (the second week’s calibrated discharge capacity is taken as C0)
[0139] 1-7) 25±2℃, charge to 4.25V with 1 / 3C0 CC-CV, and the cut-off current is 1 / 20C0;
[0140] 1-8) End;
[0141] Overcharge
[0142] 2-1) 25±2℃, 1C0 constant current charging until the cell fails, record the failure time and failure voltage;
[0143] 2-2) 25±2℃, let stand for 180min;
[0144] The results are shown in Table 1.
[0145] Table 1
[0146] Overcharge time min Charging SOC Failure voltage V Example 1 50 183% 5.5 Example 2 65 208% 5.6 Example 3 70 217% 5.6 Example 4 68 213% 5.5 Example 5 55 192% 5.6 Example 6 44 173% 5.5 Comparative Example 1 22 136% 5.5 Comparative Example 2 25 141% 5.6
[0147] As shown in Table 1, the overcharge performance of the battery cell of Example 1 is more than 30% higher than that of Comparative Example 1.
[0148] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0149] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A gel electrolyte precursor, characterized in that: Comprising a compound of structure shown in formula I, a plasticizer and a lithium salt; Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
2. The gel electrolyte precursor according to claim 1, characterized in that: The mass proportion of the compound with the structure shown in Formula I in the gel electrolyte precursor is 20% to 60%.
3. The gel electrolyte precursor according to claim 1 or 2, characterized in that: The plasticizer satisfies at least one of the conditions 1) to 2): 1) The mass proportion of the plasticizer in the gel electrolyte precursor is 20% to 60%; 2) The plasticizer is selected from at least one of succinonitrile, trans-butenedinitrile, adiponitrile, glutaronitrile, suberonitrile and sebaconitrile.
4. The gel electrolyte precursor according to claim 1 or 2, characterized in that: The lithium salt satisfies at least one of the conditions 1) to 2): 1) The mass proportion of the lithium salt in the gel electrolyte precursor is 1% to 20%; 2) The lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorooxalatoborate and lithium tetrafluoroborate; optionally, the lithium salt also includes at least one of lithium perchlorate, lithium bis(trifluoromethanesulfonylimide), lithium bis(fluorosulfonylimide), lithium bis(oxalateborate) and.
5. A gel electrolyte, characterized in that: It comprises a compound of the structure shown in formula II, a plasticizer, a lithium salt and a dispersion medium; Wherein, R1 and R2 are each independently selected from H, F, C 1-3 alkyl.
6. The gel electrolyte according to claim 5, characterized in that The dispersion medium includes an electrolyte.
7. The gel electrolyte according to claim 6, characterized in that The mass ratio of the gel electrolyte precursor to the electrolyte is (1-7):(9-3).
8. The gel electrolyte according to claim 6 or 7, characterized in that: The solvent of the electrolyte is selected from at least one of dimethyl carbonate and ethyl methyl carbonate; optionally, the solvent of the electrolyte is a mixture of dimethyl carbonate and ethyl methyl carbonate; further optionally, the volume ratio of dimethyl carbonate to ethyl methyl carbonate is 1:(1-3).
9. A method for preparing a gel electrolyte, characterized in that: The following steps are involved: The gel electrolyte precursor according to any one of claims 1 to 4 is subjected to a polymerization reaction in the presence of a dispersion medium.
10. A battery, characterized in that: A gel electrolyte comprising the gel electrolyte according to any one of claims 5 to 8 or a gel electrolyte prepared by the preparation method according to claim 9; Optionally, a positive electrode plate is also included, and the gel electrolyte is located on the positive electrode plate.
Citation Information
Cited By
High-stability gel polymer electrolyte as well as preparation method and application thereof
CN120834273A