Method for preparing lithium ion battery composite diaphragm through magnetron sputtering

The ZrO2/PE composite separator was prepared by magnetron sputtering method and dopamine self-polymerization, which solved the problem of battery short circuit and inorganic material coating thickness increase at high temperatures, and significantly improved the hydrophilicity and mechanical strength of the separator. Improves the electrochemical performance of lithium-ion batteries.

CN118943640AInactive Publication Date: 2024-11-12NANJING UNIV OF SCI & TECH

Patent Information

Application Number
CN202410977309.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When used in high temperature environments, the safety hazards of battery short circuit due to poor wetting performance and low melting point, and the thickness of the separator prepared by the traditional inorganic material coating method increases and insufficient bonding force, affecting battery performance.

Method used

The polymer microporous separator was prepared by magnetron sputtering method and composited with ZrO2 inorganic material. The hydrophilicity and mechanical strength of the separator were then improved through dopamine self-polymerization and reduced contact angle.

Benefits of technology

The hydrophilicity and mechanical strength of the separator are significantly improved, the puncture of lithium dendrites is avoided, the preparation process is simplified, the electrochemical performance loss of lithium-ion batteries is reduced, and the problems of increased thickness and insufficient binding force are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943640A_ABST
    Figure CN118943640A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a lithium ion battery composite diaphragm through magnetron sputtering. The method specifically comprises the following steps; the preparation method comprises the following steps: sputtering an inorganic material on the surface of the diaphragm by adopting a magnetron sputtering method and controlling conditions such as sputtering time and sputtering power, and then carrying out surface modification on the diaphragm through Tris-HCl (pH = 8.5) and dopamine hydrochloride to obtain the polydopamine-coated composite diaphragm. The prepared composite diaphragm is simple in process, low in cost, free of pollution and low in material consumption, the water contact angle of the modified composite diaphragm is 22 degrees which is far lower than 114 degrees of a common commercial PE diaphragm, and due to the characteristics of the magnetron sputtering process, the thickness of an inorganic material film is controllable, so that the composite diaphragm is suitable for large-scale production. The problem that the electrochemical performance of the diaphragm is damaged due to great increase of the thickness is avoided, and the diaphragm can be applied to a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of diaphragm materials for lithium ion batteries, and specifically relates to a method for preparing a composite diaphragm by plating an inorganic material on the surface of a polymer microporous diaphragm and then self-polymerizing dopamine on the diaphragm surface. Background Art

[0002] The extensive use of traditional fossil energy not only causes environmental pollution, but also exacerbates the global energy crisis. Therefore, the development of new energy is particularly important. As an environmentally friendly and efficient energy solution, lithium-ion batteries are gradually being widely used in electronic communication equipment, electric vehicles and other fields. Diaphragm material is one of the core components of lithium-ion batteries. It has two main functions: one is to isolate the positive and negative electrodes to prevent battery short circuit; the other is to provide a path for ion transmission.

[0003] Currently, commercial separators are mainly polyolefin separators, such as polyethylene separators PE, polypropylene separators PP, and polyolefin composite separators PP / PE / PP. Polyolefin separators have the advantages of good chemical stability, high mechanical strength, low cost, and simple process. However, PP and PE have low polarity and poor wettability with commonly used high-polarity solvents such as carbonates and esters. In addition, the melting point of PE separators is low, and during the operation of the battery, it may shrink due to heat due to increased temperature, resulting in battery short circuits and safety accidents. Therefore, the use of polyolefin separators in high temperature environments is limited.

[0004] Based on the characteristics of poor wetting properties and low melting point of polyolefin diaphragms, it is usually necessary to modify the diaphragms. The modification methods include surface coating, surface modification, doping with inorganic particles, etc. Among them, coating inorganic materials on the surface of the diaphragm is an effective method. Inorganic coatings such as SiO2, TiO2, Al2O3, ZrO2 and other materials can not only improve the hydrophilicity of the diaphragm, but also improve the thermal stability of the material. The traditional method of inorganic material coating is to mix inorganic particles with solvents and binders, and apply the inorganic coating on the diaphragm by scraping or dipping, and then dry it. The thickness of the diaphragm obtained by this preparation method will increase significantly, and the performance of the battery will be reduced accordingly. In addition, the bonding force between the diaphragm and the inorganic particles is weak. In the subsequent operation of the battery, problems such as shedding and clogging of pores may occur, which will have an adverse effect on the battery. Summary of the invention

[0005] Based on the defects of polyolefin membranes, the purpose of the present invention is to provide a method for preparing a composite membrane composed of a polymer membrane and an inorganic material film prepared by magnetron sputtering, and then performing surface treatment by dopamine self-polymerization. After modification, the hydrophilicity of the membrane is significantly improved and the contact angle is effectively reduced. The method is simple to operate and low in cost.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing a composite diaphragm by magnetron sputtering, wherein the polymer microporous diaphragm takes PE as an example and the inorganic material takes ZrO2 as an example, and the specific steps are as follows:

[0008] Step 1. PE microporous membrane pretreatment: soak the PE membrane in an ethanol solution for 530 minutes; then wash it with deionized water to remove the ethanol; finally dry it at 30-80°C for 5-20 hours to obtain a clean PE microporous membrane.

[0009] Step 2. Pretreatment of the target: Wipe the ZrO2 target with acetone for several times, then wipe it with 80%-98% ethanol, and blow dry.

[0010] Step 3. Magnetron sputtering treatment: Place the pretreated PE diaphragm and ZrO2 target into a magnetron sputtering coating machine, place the RF sputtering target in an argon atmosphere, and perform magnetic sputtering under the conditions of magnetic sputtering time 30-180s, magnetic sputtering power 20-100W, and sputtering pressure 0.2-1.0Pa to obtain a ZrO2 / PE composite diaphragm.

[0011] Step 4. Prepare a dopamine solution with a concentration of 2-20 mM using anhydrous methanol and Tris-HCl (pH = 8.5) as solvent (Vol: Vol = 1: 1).

[0012] The cleaned PE diaphragm is immersed in the dopamine solution for 2-24 hours, and then dried at 40-80°C for 2-24 hours to obtain a PDA / ZrO2 / PE composite diaphragm.

[0013] Compared with the prior art, the present invention has the following significant advantages:

[0014] (1) The hydrophilicity of PDA / ZrO2 / PE membrane is significantly improved, the contact angle is effectively reduced, and the electrochemical performance is improved.

[0015] (2) The ZrO2 inorganic layer improves the mechanical strength of the diaphragm and can effectively prevent lithium dendrites generated during the charging and discharging process of lithium-ion batteries from piercing the diaphragm.

[0016] (3) The present invention utilizes magnetron sputtering to prepare the composite diaphragm, which is simple and easy to control the ZrO2 loading amount.

[0017] (4) Compared with the conventional scraping or dipping method, the thickness of the ZrO2 film plated by the magnetron sputtering method adopted in the present invention is much lower than that by the conventional scraping method, which is beneficial to the electrochemical performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a diagram of the diaphragm modification mechanism.

[0019] Figure 2 is the water contact angle of commercial PE separator.

[0020] Figure 3 is the water contact angle of the composite membrane modified with dopamine. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with the embodiments and drawings.

[0022] Example 1

[0023] Step 1, pretreatment of the PE microporous membrane: soak the PE membrane in an ethanol solution for 10 minutes; then wash it with deionized water to remove the ethanol; finally dry it at 60° C. for 10 hours to obtain a cleaned PE microporous membrane.

[0024] Step 2, pretreatment of the target: wipe the ZrO2 target with acetone for several times, then wipe it with 98% ethanol, and blow dry.

[0025] Step 3, place the pretreated PE microporous membrane in a magnetron sputtering coating machine, in an argon atmosphere, adjust the sputtering power to 60 W, the sputtering pressure to 0.6 Pa, and the sputtering time to 30 s, 60 s, 90 s, 120 s, 150 s, and 180 s.

[0026] Step 4, using anhydrous methanol and Tris-HCl (pH = 8.5) as solvents (Vol: Vol = 1: 1), preparing a dopamine solution with a concentration of 10 mM, soaking the ZrO2 / PE membrane in the dopamine solution for 20 hours, and then drying it at 60°C for 24 hours to obtain a PDA / ZrO2 / PE composite membrane.

[0027] Example 2

[0028] Step 1, pretreatment of the PE microporous membrane: soak the PE membrane in an ethanol solution for 10 minutes; then wash it with deionized water to remove the ethanol; finally dry it at 60° C. for 10 hours to obtain a cleaned PE microporous membrane.

[0029] Step 2, pretreatment of the target: wipe the ZrO2 target with acetone for several times, then wipe it with 98% ethanol, and blow dry.

[0030] Step 3, placing the pretreated PE microporous membrane in a magnetron sputtering coating machine, in an argon atmosphere, adjusting the sputtering time to 120s, the sputtering pressure to 0.6Pa, and the sputtering powers to 20W, 40W, 60W, 80W, and 100W respectively.

[0031] Step 4, using anhydrous methanol and Tris-HCl (pH = 8.5) as solvents (Vol: Vol = 1: 1), prepare a dopamine solution with a concentration of 10 mM, soak the cleaned PE membrane in the dopamine solution for 20 hours, and then dry it at 60°C for 24 hours to obtain a PDA / ZrO2 / PE composite membrane.

[0032] Example 3

[0033] Step 1, pretreatment of the PE microporous membrane: soak the PE membrane in an ethanol solution for 10 minutes; then wash it with deionized water to remove the ethanol; finally dry it at 60° C. for 10 hours to obtain a cleaned PE microporous membrane.

[0034] Step 2, pretreatment of the target: wipe the ZrO2 target with acetone for several times, then wipe it with 98% ethanol, and blow dry.

[0035] Step 3, place the pretreated PE microporous membrane in a magnetron sputtering coating machine, in an argon atmosphere, adjust the sputtering time to 120s, the sputtering power to 60W, and the sputtering pressure to 0.2Pa, 0.4Pa, 0.6Pa, 0.8Pa, and 1.0Pa.

[0036] Step 4, using anhydrous methanol and Tris-HCl (pH = 8.5) as solvents (Vol: Vol = 1: 1), prepare a dopamine solution with a concentration of 10 mM, soak the cleaned PE membrane in the dopamine solution for 20 hours, and then dry it at 60°C for 24 hours to obtain a PDA / ZrO2 / PE composite membrane.

Claims

1. A method for preparing a lithium-ion battery composite diaphragm by magnetron sputtering, characterized in that: The specific steps are as follows: The diaphragm and inorganic material target are pretreated, and the pretreated diaphragm and inorganic material target are placed in an argon atmosphere, and magnetron sputtering is performed under the conditions of magnetic sputtering time 30-180s, magnetic sputtering power 20-100W, and sputtering pressure 0.2-1.0Pa. Then, the surface of the diaphragm after magnetron sputtering is modified with a dopamine hydrochloride solution to obtain a composite diaphragm.

2. The method for preparing a composite diaphragm by magnetron sputtering according to claim 1, characterized in that: The diaphragm is one or more of polyethylene (PE), polypropylene (PP), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), and polyethylene terephthalate (PET) porous membranes, and the inorganic material is one or more of Al2O3, TiO2, SiO2, ZrO2, and CeO2.

3. The method for preparing a composite diaphragm by magnetron sputtering according to claim 1, characterized in that: Pretreatment of inorganic material targets: wipe the inorganic targets repeatedly with acetone, then wipe with 80%-98% ethanol, and finally blow dry; diaphragm pretreatment: soak the diaphragm in anhydrous ethanol, take it out, wash it with deionized water and dry it.

4. The method for preparing a composite diaphragm by magnetron sputtering according to claim 1, characterized in that: Diaphragm surface modification: Prepare a dopamine solution with a concentration of 2-20 mM, the solvent is Tris-HCl (pH = 8.5): anhydrous methanol ((Vol: Vol = 1: 1), immerse the diaphragm in the dopamine solution for 2-24 hours, and then dry it at 4080°C for 2-24 hours.

5. The method for preparing a composite diaphragm by magnetron sputtering according to claim 1, characterized in that: The magnetic sputtering adopts a magnetron sputtering coating machine.

Citation Information

Patent Citations

  • Preparation method of composite membrane for lithium ion battery

    CN102407623A

  • Preparation method for inorganic / organic multilayer composite separator

    CN103066228A

  • Method for preparing CeO2 / PTFE / Nafion composite membrane by magnetron sputtering

    CN105977515A

  • Lithium supplement composite diaphragm for lithium battery, lithium battery and preparation method of lithium supplement composite diaphragm

    CN116053708A

Cited By

  • Preparation method of chitosan modified meta-aramid lithium ion battery diaphragm

    CN121484376A