Polyisocyanate composition, polyurethane resin-forming composition, film sealing material, and film module
By using a specific combination of polyisocyanate and polyurethane resin forming compositions in the film sealing material, the problem of excessive dissolution amount and viscosity of low molecular reaction products in the MDI-based polyisocyanate is solved, and low viscosity, high hardness and excellent appearance are achieved membrane sealing effect.
Patent Information
- Application Number
- CN202380030278.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-12
AI Technical Summary
When the existing MDI-based polyisocyanates are used in film sealing materials, the dissolution amount of low-molecular reaction products is difficult to control, resulting in problems of excessive viscosity or poor appearance.
The crosslinking group density and viscosity are adjusted using a polyisocyanate composition comprising diphenylmethane diisocyanate, isocyanate terminal prepolymer and isocyanate modified. , reduce the dissolution amount of low-molecular reaction products.
The film sealing material with low viscosity, excellent appearance and high hardness is achieved, reducing the dissolution of low molecular reaction products, and is suitable for sealing of hollow fiber membranes.
Smart Images

Figure BDA0005059191950000061 
Figure BDA0005059191950000062 
Figure BDA0005059191950000191
Abstract
Description
Technical Field
[0001] The present disclosure relates to a polyisocyanate composition, a polyurethane resin-forming composition, a film sealing material, and a film assembly. Background Art
[0002] In order to fix and seal membranes such as hollow fiber membranes, membrane sealing materials using diphenylmethane diisocyanate (hereinafter also referred to as MDI)-based polyisocyanates and polyols are widely used.
[0003] For example, Patent Document 1 discloses a polyurethane resin-forming composition comprising a polyisocyanate component (A) and a polyol component (B), wherein the polyisocyanate component (A) comprises a prepolymer obtained from partially dehydrated castor oil and / or partially acylated castor oil and an organic polyisocyanate.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 8-120043 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] When MDI-based polyisocyanates are used for sealing materials of glycerol-containing films, isocyanate monomers contained in MDI-based polyisocyanates react with glycerol, and low-molecular-weight reaction products in their reaction products dissolve into the liquid in contact with the film. In order to reduce the dissolution amount of the low-molecular-weight reaction products, it is necessary to reduce the amount of MDI monomers in the polyisocyanates. However, if the dissolution amount is reduced to a practical level, the amount of polyol introduced increases, and the viscosity of the polyisocyanates becomes too high. Therefore, it is difficult to take into account both low viscosity and the dissolution amount of the low-molecular-weight reaction products.
[0009] In addition, since the polyurethane resin-forming composition of Patent Document 1 uses partially dehydrated castor oil with a small amount of crosslinking components, there is a problem that the crosslinking density of the polyurethane resin is reduced, resulting in poor molding. In addition, there is also a problem that phase separation occurs inside the polyurethane resin due to the high hydrophobicity of the partially dehydrated castor oil, which sometimes causes a poor appearance of the molded product.
[0010] Therefore, one aspect of the present disclosure is to provide a polyisocyanate composition and a polyurethane resin-forming composition with low viscosity that have little dissolution, are helpful for producing a film sealing material with high hardness and excellent appearance. In addition, one aspect of the present disclosure is to provide a film sealing material and a film assembly using the above-mentioned polyurethane resin-forming composition.
[0011] Solutions for solving problems
[0012] According to each aspect of the present disclosure, the following embodiments [1] to
[13] are provided.
[0013] [1]: A polyisocyanate composition comprising a polyisocyanate (A),
[0014] The polyisocyanate (A) comprises:
[0015] Diphenylmethane diisocyanate (a1),
[0016] Isocyanate-terminated prepolymer (a2), and
[0017] Isocyanate-modified product (a3),
[0018] The isocyanate-terminated prepolymer (a2) is a reaction product of a polyisocyanate (a2-1) and a polyol (a2-2).
[0019] The polyisocyanate (a2-1) comprises diphenylmethane diisocyanate (a2-1-1) and a modified isocyanate (a2-1-2).
[0020] The modified isocyanate (a2-1-2) and the modified isocyanate (a3) are at least one selected from the group consisting of carbodiimide-modified diphenylmethane diisocyanate and uretonimine-modified diphenylmethane diisocyanate,
[0021] The modified isocyanate (a3) is a modified diphenylmethane diisocyanate.
[0022] The content of the modified isocyanate (a2-1-2) in the polyisocyanate (a2-1) is 4.5 to 15% by mass.
[0023] [2]: The polyisocyanate composition according to [1], wherein the modified isocyanate (a3) comprises at least one selected from the group consisting of carbodiimide-modified diphenylmethane diisocyanate and uretonimine-modified diphenylmethane diisocyanate.
[0024] [3]: The polyisocyanate composition according to [1] or [2], wherein the total content of the structural unit derived from the modified isocyanate (a2-1-2) and the modified isocyanate (a3) in the polyisocyanate (A) is 4.5 to 15% by mass.
[0025] [4]: The polyisocyanate composition according to any one of [1] to [3], wherein in the isocyanate-terminated prepolymer (a2), the content ratio of the structural unit derived from 4,4'-diphenylmethane diisocyanate in the structural unit derived from diphenylmethane diisocyanate is 50 to 80%.
[0026] [5]: The polyisocyanate composition according to any one of [1] to [4], wherein in the isocyanate-terminated prepolymer (a2), the total content of the structural units derived from 2,2'-diphenylmethane diisocyanate and the structural units derived from 2,4'-diphenylmethane diisocyanate in the structural units derived from diphenylmethane diisocyanate is 20 to 50%.
[0027] [6]: A polyurethane resin-forming composition comprising:
[0028] The polyisocyanate composition according to any one of [1] to [5], and
[0029] Polyol (B).
[0030] [7]: The polyurethane resin-forming composition according to [6], wherein
[0031] The aforementioned polyol (B) comprises:
[0032] At least one polyol (b1) selected from the group consisting of castor oil, partially dehydrated castor oil and castor oil-modified polyol; and
[0033] An amine compound (b2) having two or more hydroxyl groups.
[0034] [8]: The polyurethane resin-forming composition according to [7], wherein the content of the amine compound (b2) in the polyol (B) is 30% by mass or less.
[0035] [9]: The polyurethane resin-forming composition according to any one of [6] to [8], wherein the crosslinking group density is 0.9 mmol / g or more.
[0036]
[10] : The polyurethane resin-forming composition according to any one of [6] to [9], which is used for a film sealing material.
[0037]
[11] : A film sealing material comprising a cured product of the polyurethane resin-forming composition according to any one of [6] to
[10] .
[0038]
[12] : A membrane module comprising:
[0039] Main body,
[0040] Membranes, and
[0041] a membrane sealing material for sealing the gap between the main body and the membrane,
[0042] The aforementioned film sealing material is the film sealing material described in
[11] .
[0043]
[13] : The membrane module according to
[12] , wherein
[0044] The aforementioned membrane comprises a plurality of hollow fiber membranes,
[0045] The membrane sealing material seals a gap between the main body and at least a part of the hollow fiber membranes and at least a part of a gap between the hollow fiber membranes.
[0046] Effects of the Invention
[0047] According to one embodiment of the present disclosure, it is intended to provide a polyisocyanate composition and a polyurethane resin-forming composition with low viscosity that have little elution, are helpful in producing a film sealing material with high hardness and excellent appearance. In addition, it is intended to provide a film sealing material and a film assembly using the above-mentioned polyurethane resin-forming composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a schematic diagram showing an example of the configuration of a membrane module according to one embodiment of the present disclosure. DETAILED DESCRIPTION
[0049] Hereinafter, exemplary embodiments of each mode for implementing the present disclosure will be described in further detail. However, the present disclosure is not limited to the following embodiments.
[0050] In this specification, the numerical range shown by "~" indicates that the range includes the numerical values recorded before and after "~" as the minimum value and the maximum value, respectively. Within the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. In addition, the upper limit and lower limit recorded separately can be combined arbitrarily.
[0051] [Polyisocyanate composition]
[0052] The polyisocyanate composition according to one embodiment of the present disclosure includes a polyisocyanate (A), wherein the polyisocyanate (A) includes diphenylmethane diisocyanate (a1), an isocyanate-terminated prepolymer (a2), and a modified isocyanate (a3).
[0053] <Diphenylmethane diisocyanate (a1)>
[0054] Diphenylmethane diisocyanate (a1) may be any diphenylmethane diisocyanate (hereinafter referred to as MDI) that is commonly available. MDI may include isomers such as 4,4'-MDI, 2,4'-MDI, and 2,2'-MDI. In this specification, 4,4'-MDI may be referred to as a main component, and 2,4'-MDI and 2,2'-MDI may be referred to as isomeric components.
[0055] In diphenylmethane diisocyanate (a1), the content of 2,2′-MDI may be 0% to 5% by mass, the content of 2,4′-MDI may be 0% to 95% by mass, and the content of 4,4′-MDI may be 5% to 100% by mass.
[0056] The content of diphenylmethane diisocyanate (a1) in the polyisocyanate (A) may be, for example, 20% by mass or more and 55% by mass or less, preferably 25% by mass or more and 50% by mass or less, and more preferably 30% by mass or more and 45% by mass or less.
[0057] <Isocyanate-terminated prepolymer (a2)>
[0058] The isocyanate-terminated prepolymer (a2) is a reaction product of a polyisocyanate (a2-1) and a polyol (a2-2). The reaction of the polyisocyanate (a2-1) and the polyol (a2-2) may be a urethanization reaction.
[0059] The polyisocyanate (a2-1) contains diphenylmethane diisocyanate (a2-1-1) and a modified isocyanate (a2-1-2).
[0060] The diphenylmethane diisocyanate (a2-1-1) may be any conventionally available diphenylmethane diisocyanate (hereinafter also referred to as MDI). In the diphenylmethane diisocyanate (a2-1-1), the content of 2,2'-MDI may be 0% by mass or more and 5% by mass or less, the content of 2,4'-MDI may be 0% by mass or more and 95% by mass or less, and the content of 4,4'-MDI may be 5% by mass or more and 100% by mass or less.
[0061] The content of diphenylmethane diisocyanate (a2-1-1) in the polyisocyanate (a2-1) can be, for example, 85% by mass or more and 95.5% by mass or less, preferably 85% by mass or more and 95% by mass or less, and more preferably 85.5% by mass or more and 94.5% by mass or less. Within this range, the appearance and low dissolution property of the polyurethane resin are more excellent.
[0062] The modified isocyanate (a2-1-2) is at least one modified product selected from the group consisting of carbodiimide-modified diphenylmethane diisocyanate and uretonimine-modified diphenylmethane diisocyanate.
[0063] Carbodiimide-modified diphenylmethane diisocyanate is a modified body formed by condensation between isocyanate groups of MDI accompanied by CO2 generation, and can be, for example, a compound shown in the following formula (1-1). In addition, uretonimine-modified diphenylmethane diisocyanate is a modified body formed by the reaction of carbodiimide-modified diphenylmethane diisocyanate and MDI, and can be, for example, a compound shown in the following formula (1-2).
[0064] RN=C=NR (1-1)
[0065]
[0066] In formula (1-1) and formula (1-2), R represents a group represented by formula (2), preferably a group represented by formula (2-1), formula (2-2-1), formula (2-2-2) or formula (2-3); more preferably a group represented by formula (2-1), formula (2-2-1) or formula (2-2-2); further preferably a group represented by formula (2-1).
[0067]
[0068] The content of the modified isocyanate (a2-1-2) in the polyisocyanate (a2-1) is 4.5% by mass or more and 15% by mass or less, preferably 5% by mass or more and 15% by mass or less, and more preferably 5.5% by mass or more and 14.5% by mass or less. Within this range, the polyurethane resin has excellent appearance and low solubility.
[0069] Polyisocyanate (a2-1) can comprise polyisocyanates other than diphenylmethane diisocyanate (a2-1-1) and isocyanate-modified body (a2-1-2).For example, polyisocyanate (a2-1) can further comprise carbamate-modified body, polymer, urea-modified body, allophanate-modified body, biuret-modified body, uretonimine-modified body or uretdione-modified body etc. of diphenylmethane diisocyanate.
[0070] The total content of diphenylmethane diisocyanate (a2-1-1) and modified isocyanate (a2-1-2) in the polyisocyanate (a2-1) may be, for example, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more.
[0071] The polyol (a2-2) is not particularly limited as long as it is a compound having two or more hydroxyl groups. Examples of the polyol (a2-2) include castor oil, partially dehydrated castor oil, castor oil-modified polyols, low molecular weight polyols, polyether polyols, polyester polyols, polylactone polyols, polyolefin polyols and the like.
[0072] Examples of castor oil-modified polyols include linear or branched castor oil-modified polyols obtained by reacting castor oil or castor oil fatty acid with at least one polyol selected from the group consisting of low molecular weight polyols and polyether polyols. Specific examples include diglycerides and monoglycerides of castor oil fatty acids; monoesters, diesters, and triesters of castor oil fatty acids and trimethylolalkanes; and monoesters, diesters, and triesters of castor oil fatty acids and polypropylene glycol.
[0073] It should be noted that the main component of castor oil is triglyceride of ricinoleic acid, and castor oil includes hydrogenated castor oil. In addition, the main component of castor oil fatty acid is ricinoleic acid, and castor oil fatty acid includes hydrogenated castor oil fatty acid.
[0074] Examples of the trimethylolalkane include trimethylolmethane, trimethylolethane, trimethylolpropane, trimethylolbutane, trimethylolpentane, trimethylolhexane, trimethylolheptane, trimethyloloctane, trimethylolnonane, and trimethyloldecane.
[0075] The number average molecular weight of the castor oil-modified polyol is preferably 400 to 3000, more preferably 500 to 2500. When the number average molecular weight of the castor oil-modified polyol is 400 to 3000, a cured resin having more excellent physical properties, particularly mechanical properties, required for a film sealing material can be obtained.
[0076] In addition, in this specification, the number average molecular weight shows the value measured by the method shown below.
[0077] <Determination of number average molecular weight>
[0078] The number average molecular weight was determined by GPC measurement under the following conditions and method.
[0079] (Measurement conditions of number average molecular weight)
[0080] (1) Measurement device: "HLC-8120 (trade name)" (manufactured by Tosoh Corporation)
[0081] (2) Column: Four columns each filled with two TSKgel G2000HXL and two TSKgel G3000HXL (both trade names, manufactured by Tosoh Corporation) as a filler were connected in series.
[0082] (3) Column temperature: 40°C
[0083] (4) Detector: RI (refractive index) meter
[0084] (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min, 40°C)
[0085] (6) Calibration curve: A calibration curve was obtained using the following trifunctional polypropylene polyols (all manufactured by Sanyo Chemical Industries, Ltd.).
[0086] "Sannix GP-250" (number average molecular weight = 250)
[0087] "Sannix GP-400" (number average molecular weight = 400)
[0088] "Sannix GP-600" (number average molecular weight = 600)
[0089] "Sannix GP-1000" (number average molecular weight = 1000)
[0090] "Sannix GP-3000" (number average molecular weight = 3000)
[0091] "Sannix GP-4000" (number average molecular weight = 4000)
[0092] "Sannix GP-5000" (number average molecular weight = 5000)
[0093] (7) Sample solution: 0.05 g sample in 10 mL THF
[0094] The average hydroxyl value of castor oil, partially dehydrated castor oil and castor oil modified polyol is preferably 20 mgKOH / g or more and 300 mgKOH / g or less, and more preferably 40 mgKOH / g or more and 250 mgKOH / g or less. If the average hydroxyl value is 20 mgKOH / g or more and 300 mgKOH / g or less, a cured resin having excellent physical properties, especially mechanical properties, required by the membrane sealing material can be formed. In addition, the productivity of the membrane sealing material and the productivity of the hollow fiber membrane module can be improved.
[0095] In addition, in this specification, the average hydroxyl value shows the value measured by the method shown below.
[0096] <Measurement of Hydroxyl Value>
[0097] The hydroxyl value is a value measured by a method using an acetylating agent in accordance with JIS K1557-1.
[0098] Examples of low molecular weight polyols include divalent polyols such as ethylene glycol, diethylene glycol, propylene glycol, 1,2-, 1,3- or 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentyl glycol, and hydrogenated bisphenol A; and trivalent to octavalent polyols such as glycerol, trimethylolpropane, hexanetriol, pentaerythritol, sorbitol, and sucrose. The number average molecular weight of the low molecular weight polyol is preferably 50 or more and 200 or less.
[0099] Examples of polyether polyols include: alkylene oxide (alkylene oxides having 2 to 8 carbon atoms, such as ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above-mentioned low molecular weight polyols, and ring-opening polymers of alkylene oxides, etc. Specifically, examples include: polypropylene glycol, polyethylene glycol, polytetramethylene ether glycol, and copolymers of ethylene oxide and propylene oxide, etc. From the viewpoint of further excellent molding processability when manufacturing film sealing materials, the number average molecular weight of the polyether polyol is preferably 200 or more and 7000 or less, and more preferably 500 or more and 5000 or less.
[0100] Examples of the polyester polyol include polyester polyols obtained by polycondensation of polycarboxylic acid and polyol.
[0101] Examples of the polycarboxylic acid used for the polyester polyol include aliphatic saturated and unsaturated polycarboxylic acids such as adipic acid, azelaic acid, dodecanedioic acid, maleic acid, fumaric acid, itaconic acid, dimerized linoleic acid, phthalic acid, isophthalic acid, and terephthalic acid, and aromatic polycarboxylic acids.
[0102] Examples of the polyol used for the polyester polyol include the above-mentioned low molecular weight polyols and polyether polyols.
[0103] The number average molecular weight of the polyester polyol is preferably 200 to 5000, more preferably 500 to 3000. When the number average molecular weight of the polyester polyol is 200 to 5000, the molding processability when formed into a film sealing material is particularly excellent.
[0104] As polylactone polyols, for example, polyols obtained by addition polymerization of a polymerization initiator of a diol or triol with ε-caprolactone, α-methyl-ε-caprolactone, ε-methyl-ε-caprolactone, β-methyl-δ-valerolactone, etc., in the presence of a catalyst such as an organic metal compound, a metal chelate compound, or a fatty acid metal acyl compound can be cited. The number average molecular weight of the polylactone polyol is preferably 200 to 5000, and more preferably 500 to 3000. If the number average molecular weight of the polylactone polyol is 200 to 5000, the molding processability when forming a film sealing material is particularly excellent.
[0105] Examples of polyolefin polyols include polybutadiene polyols having hydroxyl groups introduced into the ends of polybutadiene or copolymers of butadiene and styrene or acrylonitrile. In addition, examples include polyetherester polyols obtained by addition reaction of polyesters having carboxyl groups and hydroxyl groups at the ends with alkylene oxides such as ethylene oxide and propylene oxide.
[0106] Among them, the polyol (a2-2) is preferably castor oil, partially dehydrated castor oil or castor oil-modified polyol in view of compatibility with the polyol (B), and more preferably contains partially dehydrated castor oil from the viewpoint of low solubility.
[0107] The isocyanate-terminated prepolymer (a2) is a reaction product of a polyisocyanate (a2-1) and a polyol (a2-2). The reaction of the polyisocyanate (a2-1) and the polyol (a2-2) may be a commonly performed urethanization reaction.
[0108] The reaction conditions of the polyisocyanate (a2-1) and the polyol (a2-2) are not particularly limited. The reaction temperature may be, for example, 40° C. or higher and 80° C. or lower.
[0109] In the isocyanate-terminated prepolymer (a2), the content ratio of the structural unit derived from 4,4'-diphenylmethane diisocyanate in the structural unit derived from diphenylmethane diisocyanate is preferably 50% by mass or more and 80% by mass or less, more preferably 52% by mass or more and 79% by mass or less, and more preferably 54% by mass or more and 79% by mass or less. When it is within these ranges, the viscosity of the polyisocyanate (A) becomes lower, and excessive polymerization can be further suppressed.
[0110] In the isocyanate-terminated prepolymer (a2), the content ratio of the structural unit derived from the isomeric component containing 4,4'-diphenylmethane diisocyanate (4,4'-MDI) and 2,2'-diphenylmethane diisocyanate (2,2'-MDI) in the structural unit derived from diphenylmethane diisocyanate is preferably 20 mass % or more and 50 mass % or less, more preferably 21 mass % or more and 48 mass % or less, more preferably 21 mass % or more and 46 mass % or less. When it is within these ranges, the viscosity of the polyisocyanate (A) becomes lower, and excessive polymerization can be further suppressed.
[0111] The content of the isocyanate-terminated prepolymer (a2) in the polyisocyanate (A) may be, for example, 30% by mass or more and 75.5% by mass or less, preferably 35% by mass or more and 70.5% by mass or less, and more preferably 40% by mass or more and 65.5% by mass or less.
[0112] <Isocyanate modified product (a3)>
[0113] Isocyanate modified body (a3) is a modified body of diphenylmethane diisocyanate, preferably comprising at least one modified body (a3-1) selected from the group consisting of carbodiimide modified diphenylmethane diisocyanate and uretonimine modified diphenylmethane diisocyanate. As carbodiimide modified diphenylmethane diisocyanate and uretonimine modified diphenylmethane diisocyanate, the same material as isocyanate modified body (a2-1-2) can be illustrated.
[0114] The isocyanate-modified product (a3) may further include a urethane-modified product, a polymer, a urea-modified product, an allophanate-modified product, a biuret-modified product, a uretonimine-modified product, or a uretdione-modified product of diphenylmethane diisocyanate.
[0115] The content of the modified product (a3-1) in the isocyanate modified product (a3) may be, for example, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more.
[0116] In the polyisocyanate (A), the total content of the structural unit derived from the isocyanate modified body (a2-1-2) and the modified body (a3-1) is preferably 4.5% by mass or more and 15% by mass or less, more preferably 5.0% by mass or more and 15% by mass or less, and further preferably 5.5% by mass or more and 14.5% by mass or less. When it is within these ranges, the appearance and low dissolution of the polyurethane resin are excellent.
[0117] In the polyisocyanate (A), the total content of the structural unit derived from the isocyanate modified body (a2-1-2) and the isocyanate modified body (a3) is preferably 4.5% by mass or more and 15% by mass or less, more preferably 5.0% by mass or more and 15% by mass or less, and further preferably 5.5% by mass or more and 14.5% by mass or less. When it is within these ranges, the appearance and low dissolution of the polyurethane resin are excellent.
[0118] The polyisocyanate (A) may further contain a polyisocyanate other than the diphenylmethane diisocyanate (a1), the isocyanate-terminated prepolymer (a2) and the isocyanate-modified product (a3).
[0119] The total content of diphenylmethane diisocyanate (a1), isocyanate-terminated prepolymer (a2) and isocyanate modified product (a3) in the polyisocyanate (A) may be, for example, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more.
[0120] The content of the isocyanate group of the polyisocyanate (A) is preferably 13% by mass or more and 21% by mass or less, more preferably 13.5% by mass or more and 20.5% by mass or less, and particularly preferably 14% by mass or more and 20% by mass or less. When it is within these ranges, the molding processability and adhesive strength of the polyurethane resin are further excellent.
[0121] [Polyurethane resin forming composition]
[0122] The polyurethane resin-forming composition according to one embodiment of the present disclosure includes the above-mentioned polyisocyanate composition and a polyol (B).
[0123] <Polyol (B)>
[0124] The polyol (B) may be a compound having two or more hydroxyl groups. The polyol (B) preferably comprises at least one polyol (b1) selected from the group consisting of castor oil, partially dehydrated castor oil and castor oil-modified polyol, and an amine compound (b2) having two or more hydroxyl groups.
[0125] Examples of the polyol (b1) include the castor oil, partially dehydrated castor oil, and castor oil-modified polyol exemplified as the polyol (a2-2).
[0126] The content of the polyol (b1) in the polyol (B) is preferably 70% by mass or more, more preferably 70% by mass or more and 95% by mass or less, further preferably 75% by mass or more and 90% by mass or less.
[0127] Examples of the amine compound (b2) include: linear or branched alkyldiethanolamines such as butyldiethanolamine, hexyldiethanolamine, octyldiethanolamine, lauryldiethanolamine, myristyldiethanolamine, hexadecyldiethanolamine, and stearyldiethanolamine; low molecular weight polyamines; and amine compounds such as low molecular weight amino alcohols.
[0128] More specifically, the amine compounds include: propylene oxide or ethylene oxide addition products of ethylenediamine, i.e., oxyalkylated derivatives of amino compounds such as N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine and N,N,N',N'-tetrakis[2-hydroxyethyl]ethylenediamine; monoethanolamine, diethanolamine, triethanolamine; and amino alcohol derivatives such as N-methyl-N,N'-diethanolamine.
[0129] Among them, propylene oxide or ethylene oxide adducts of amino compounds such as ethylenediamine are preferred, and N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine is most preferred. By using N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine, further effects are exerted due to improved processability during molding and reduced elution.
[0130] The content of the amine compound (b2) in the polyol (B) is preferably 30% by mass or less, more preferably 5% by mass or more and 30% by mass or less, and further preferably 10% by mass or more and 25% by mass or more. When the proportion of the amine compound (b2) in the polyol (B) is 30% by mass or less, the reactivity is further suppressed from becoming too high, the operability is further improved to ensure the filling property, and the hardness of the obtained film sealing material is further suppressed from becoming too high. In addition, when the proportion of the amine compound (b2) in the polyol (B) is 5% by mass or more, the amine compound (b2) performs its function better and exerts a further effect.
[0131] The polyol (B) may further contain a polyol (b3) other than the polyol (b1) and the amine compound (b2). Examples of the polyol (b3) include the various polyols exemplified as the polyol (a2-2) described above.
[0132] The total content of the polyol (b1) and the amine compound (b2) in the polyol (B) may be, for example, 50% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more.
[0133] The hydroxyl value of the polyol (B) is preferably 50 mgKOH / g or more and 1000 mgKOH / g or less, and is more preferably 75 mgKOH / g or more and 750 mgKOH / g or less from the viewpoint of easy handling of the polyol (B). From the viewpoint of excellent molding processability and adhesive strength of the polyurethane resin, the hydroxyl value of the polyol (B) is further preferably 100 mgKOH / g or more and 500 mgKOH / g or less.
[0134] The viscosity of the polyol (B) at 25°C is preferably 100 mPa·s or more and 6000 mPa·s, and is more preferably 150 mPa·s or more and 4000 mPa·s or less from the viewpoint of easy handling of the polyol (B). From the viewpoint of excellent molding processability of the polyurethane resin, the viscosity of the polyol (B) at 25°C is further preferably 200 mPa·s or more and 2000 mPa·s or less.
[0135] In order to further reduce the low-molecular-weight reaction products of MDI and glycerin, the content of the MDI monomer is preferably 25% by mass or less based on the total amount of the polyurethane resin-forming composition.
[0136] The polyurethane resin forming composition may be a two-component type. That is, the polyurethane resin forming composition may contain, for example: a first component including a polyisocyanate composition, and a second component including a polyol (B). Such a polyurethane resin forming composition may be formed into a polyurethane resin by mixing the first component and the second component.
[0137] For the polyurethane resin-forming composition, the viscosity after 60 seconds from the time when the polyisocyanate composition and the polyol (B) begin to be mixed (for example, the first agent and the second agent are mixed) (also called mixed viscosity) is preferably 400 mPa·s or more and 2100 mPa·s or less, and more preferably 500 mPa·s or more and 1800 mPa·s or less.
[0138] From the viewpoint of further suppressing elution into a solvent, the crosslinking group density of the polyurethane resin-forming composition is preferably 0.9 mmol / g or more relative to the total mass of the polyisocyanate (A) and the polyol (B), and is more preferably 0.9 mmol / g or more and 1.2 or less from the viewpoint of molding processability.
[0139] It should be noted that the crosslinking group density refers to the total content density of the groups that can form crosslinks and the groups that have formed crosslinks.
[0140] Therefore, if a trifunctional polyol (such as glycerol) is used as an example for explanation, since one hydroxyl group in one molecule forms a crosslink and the remaining two hydroxyl groups do not participate in the crosslink, in this case, the number of crosslinking groups is 1. That is, in the case of a polyurethane resin-forming composition containing a trifunctional polyol, since the trifunctional polyol has one crosslinking group, the content of the crosslinking group derived from the trifunctional polyol has the same meaning as the content of the trifunctional polyol.
[0141] The polyurethane resin-forming composition of one embodiment of the present disclosure can suppress the dissolution amount of the low molecular weight reaction product of MDI and glycerin, has excellent moldability, and helps to produce a film sealing material with excellent appearance. That is, the polyurethane resin-forming composition can be a polyurethane resin-forming composition for film sealing materials suitable for film sealing material applications.
[0142] <Method for producing polyisocyanate composition>
[0143] A method for producing a polyisocyanate composition according to one embodiment of the present disclosure includes:
[0144] Obtaining the isocyanate-terminated prepolymer (a2) which is a reaction product of the polyisocyanate (a2-1) and the polyol (a2-2); and
[0145] Diphenylmethane diisocyanate (a1), an isocyanate-terminated prepolymer (a2), and an isocyanate-modified product (a3) are mixed to obtain a polyisocyanate composition containing a polyisocyanate (A).
[0146] The polyisocyanate (a2-1), polyol (a2-2), isocyanate-terminated prepolymer (a2), diphenylmethane diisocyanate (a1) and isocyanate-modified product (a3) may be the same as the components in the above-mentioned polyisocyanate composition, respectively. In addition, their blending ratio may be the same as the blending ratio of the components in the above-mentioned polyisocyanate composition.
[0147] <Method for producing polyurethane resin-forming composition>
[0148] A method for producing a polyurethane resin-forming composition according to one embodiment of the present disclosure includes:
[0149] Obtaining the reaction product of the polyisocyanate (a2-1) and the polyol (a2-2), namely, the isocyanate-terminated prepolymer (a2);
[0150] Mixing diphenylmethane diisocyanate (a1), an isocyanate-terminated prepolymer (a2), and an isocyanate-modified product (a3) to obtain a polyisocyanate composition containing a polyisocyanate (A); and
[0151] Prepare polyol (B).
[0152] The polyisocyanate (a2-1), polyol (a2-2), isocyanate-terminated prepolymer (a2), diphenylmethane diisocyanate (a1), isocyanate-modified product (a3) and polyol (B) may be the same as the components in the above-mentioned polyurethane resin-forming composition. In addition, the mixing ratio thereof may be the same as the mixing ratio of the components in the above-mentioned polyurethane resin-forming composition.
[0153] <Film sealing material (second aspect)>
[0154] The film sealing material according to one embodiment of the present disclosure includes a cured product of the polyurethane resin-forming composition.
[0155] The film sealing material can be suitably formed by reacting and curing the polyisocyanate (A) and the polyol (B) under the temperature condition of 0°C to 100°C, preferably 20°C to 80°C, more preferably 30°C to 60°C.
[0156] The gelling time of the film sealing material can be shortened by molding in a high temperature region, but since it is easy to cause molding shrinkage, the molding shrinkage can be suppressed by lowering the reaction temperature by adding a catalyst.
[0157] <Membrane module (third embodiment)>
[0158] A membrane module according to one embodiment of the present disclosure includes: a main body; a membrane; and a membrane sealing material that seals a gap between the main body and the membrane.
[0159] The membrane may include a plurality of hollow fiber membranes. In this case, the membrane sealing material preferably seals a gap between the main body and at least a part of the hollow fiber membranes, and at least a part of the gaps between the hollow fiber membranes.
[0160] Next, a membrane module according to an embodiment of the present disclosure will be described in further detail with reference to the drawings.
[0161] Figure 1 This is a schematic diagram showing an example of the structure of a membrane module according to one embodiment of the present disclosure.
[0162] Figure 1 The membrane module (hollow fiber membrane module) 100 shown includes a housing (main body) 11, the interior of which is filled with a plurality of hollow fiber membranes (membranes) 13. For example, in the case of a hollow fiber membrane module used as a dialyzer, several thousand to several tens of thousands of hollow fiber membranes are filled.
[0163] The housing 11 has a cylindrical shape. Figure 1The membrane sealing material 19 is provided at the left and right ends of the housing 11. The membrane sealing material fills and seals the gaps between the hollow fiber membranes 13 and the gaps between the hollow fiber membranes 13 and the inner wall of the housing 11, and bundles the plurality of hollow fiber membranes 13.
[0164] In addition, the side of the shell 11 is provided with a first fluid inlet 15 and a first fluid outlet 17, by means of which the first fluid (gas or liquid) flows in and out of the shell 11. The first fluid flowing in from the first fluid inlet 15 contacts the plurality of hollow fiber membranes 13 filled in the shell 11, and is discharged from the first fluid outlet 17 through the gaps (outside the hollow fiber membranes). It should be noted that there is no membrane sealing material 19 inside the hollow fiber membrane 13, so the second fluid (gas or liquid) flows in and out of the hollow fiber membrane 13 by means of a second inlet (one end side) and a second outlet (the other end side) provided with a cover member not shown in the figure. Then, the first fluid is contacted with the second fluid by means of the hollow fiber membrane 13, thereby generating a substance from one fluid to another fluid (or further from another fluid to one fluid). For example, in the case of a hollow fiber membrane type dialyzer, the dialysate contacts the blood, so that waste and excess water in the blood move to the dialysate.
[0165] It should be noted that Figure 1 The membrane assembly 100 shown is a structure having a plurality of hollow fiber membranes 13 and a membrane sealing material 19 for sealing the gaps at both ends thereof, but the membrane assembly of this embodiment is not limited to the above structure at all. For example, it may be a plurality of or a single membrane having various shapes such as a flat membrane or a spiral membrane. In addition, the membrane sealing material is not limited to a structure provided at both ends of the membrane, and may be provided only at a portion of the membrane (one end if it is a hollow fiber), or may be provided at the entire end of the membrane, such as the entire outer edge of a flat membrane. Furthermore, the sealing material may be a structure provided at a portion other than the end of the membrane and sealed. In addition, Figure 1 The housing 11 of the membrane module 100 shown has a cylindrical shape, but may have any shape other than a cylindrical shape.
[0166] The membrane assembly 100 uses the above-mentioned membrane sealing material polyurethane resin forming composition to seal the gaps between the hollow fiber membranes 13 at the end of the bundle of multiple hollow fiber membranes 13, and solidifies the composition to form the above-mentioned membrane sealing material (the gaps between the hollow fiber membranes are sealed by this membrane sealing material).
[0167] The membrane module of one embodiment of the present disclosure suppresses the production of extracts well and can therefore be suitably used as a medical or water treatment module. Specific examples of the membrane module include plasma separation devices, artificial lungs, artificial kidneys, artificial livers, and domestic / industrial water treatment devices.
[0168] Example
[0169] Hereinafter, the present invention will be described based on Examples, but the present invention is not limited to these Examples. It should be noted that "%" below means "mass %" unless otherwise specified.
[0170] The following components were used in Examples and Comparative Examples.
[0171] [Polyisocyanate (A)]
[0172] a-1;
[0173] 4,4'-MDI (manufactured by Tosoh Corporation, product name Millionate MT, isocyanate group content = 33.6%, carbodiimide / uretonimine modified body content = 0%, isomers = about 1%, crosslinking group density = 0 mmol / g)
[0174] a-2;
[0175] Mixture of 2,4'-MDI and 4,4'-MDI (manufactured by Tosoh Corporation, product name Millionate NM, isocyanate group content = 33.6%, carbodiimide / uretonimine modified body content = 0%, isomers = about 55%, crosslinking group density = 0 mmol / g)
[0176] a-3;
[0177] Carbodiimide-modified 4,4'-MDI (manufactured by Tosoh Corporation, product name Millionate MTL-C, isocyanate group content = 28.6%, carbodiimide / uretonimine-modified body content = 30%, isomers = about 1%, crosslinking group density = 0.45 mmol / g)
[0178] [Polyol (B)]
[0179] b-1;
[0180] Castor oil (manufactured by Ito Oil Products Co., Ltd., product name URIC H-30, OHV = 160 mgKOH / g, viscosity (25°C) = 690 mPa·s, crosslinking group density = 0.74 mmol / g)
[0181] b-2;
[0182] Partially dehydrated castor oil (manufactured by Ito Oil Products Co., Ltd., molecular weight 950, OHV = 119 mgKOH / g, viscosity (25°C) = 420 mPa·s, crosslinking group density = 0 mmol / g)
[0183] b-3;
[0184] Polymerized castor oil (manufactured by Ito Oil Products Co., Ltd., product name POLYCASTOR #30, OHV = 155 mgKOH / g, viscosity (25°C) = 4800 mPa·s, crosslinking group density = 1.84 mmol / g)
[0185] b-4;
[0186] N,N,N',N'-Tetrakis[2-hydroxypropyl]ethylenediamine
[0187] (ADEKA Corporation, product name EDP-300, OHV = 760 mgKOH / g, viscosity (25°C) = 50000 mPa·s, crosslinking group density = 2.63 mmol / g)
[0188] b-5;
[0189] N-Lauryl diethanolamine
[0190] (Manufactured by Kao Corporation, product name AMIET 102, OHV = 394 mgKOH / g, viscosity (25°C) = 100 mPa·s, crosslinking group density = 0 mmol / g)
[0191] (Calculation method of cross-linking group density)
[0192] The crosslinking group density in the table below was calculated using the following formula based on the number of functional groups, hydroxyl value, and number average molecular weight obtained by GPC measurement disclosed by each raw material manufacturer. Note that GPC measurement was performed under the conditions described below in <Measurement of MDI Content>.
[0193]
[0194] <Example A-1: Preparation of polyisocyanate composition>
[0195] The raw materials shown in step 1 of Table 1 were added in the mixing ratio described in Table 1, and stirred and mixed at 70° C. for 4 hours to react to obtain an isocyanate-terminated prepolymer (a2). After the reaction, the raw materials shown in step 2 of Table 1 were added in the mixing ratio described in Table 1, and stirred and mixed at 55° C. for 2 hours to obtain a polyisocyanate composition (A-1) containing a polyisocyanate (A).
[0196] <Examples A-2 to A-7>
[0197] A polyisocyanate composition was obtained in the same manner as in Example A-1 except that the blending ratio of each raw material was changed to the blending ratio described in Table 1 or Table 2.
[0198] <Comparative Examples A'-1 to A'-3>
[0199] Except having changed the compounding ratio of each raw material into the compounding ratio described in Table 3, it carried out similarly to Example A-1, and obtained the polyisocyanate composition.
[0200] <Comparative Examples A'-4 to A'-6>
[0201] The raw materials shown in Table 4 were added at the mixing ratio described in Table 4, and stirred and mixed at 70° C. for 4 hours to allow the mixture to react, thereby obtaining a polyisocyanate composition.
[0202] [Table 1]
[0203]
[0204] [Table 2]
[0205]
[0206] [Table 3]
[0207]
[0208] [Table 4]
[0209]
[0210] In the table, the MDI content represents the value measured by the following method. In addition, in the table, the modified MDI content is the total amount of the modified MDI mixed in step 1 and the modified MDI mixed in step 2, which can also be called the sum of the content of the isocyanate modified body and the content of the structural unit derived from the isocyanate modified body in the prepolymer. In addition, in the table, the NCO content is the content of the isocyanate group in the composition, which is measured by the following method. In addition, in the table, the viscosity at 25°C is measured by the following method.
[0211] <Determination of MDI content>
[0212] The MDI content (mass %) was measured by GPC (Gel Permeation Chromatography) and determined based on the following conditions and method.
[0213] ·Measurement conditions
[0214] (1) Measurement device: "HLC-8120 (trade name)" (manufactured by Tosoh Corporation)
[0215] (2) Column temperature: 40°C
[0216] (3) Detector: RI (refractive index) meter
[0217] (4) Column: Columns filled with three types of fillers, namely, TSKgel G3000HXL, TSKgel G2000HXL, and TSKgel G1000HXL (all trade names, manufactured by Tosoh Corporation), were connected in series and measured.
[0218] (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min, 40°C)
[0219] (6) Standard curve: The standard curve was obtained using the following grade of polystyrene (TSK standard POLYSTYRENE).
[0220] F-2(1.81×10 4 )F-1(1.02×10 4 )A-5000(5.97×10 3 )A-2500(2.63×10 3 )A-500(Mw=6.82×10 2 , 5.78×10 2 4.74×10 2 3.70×10 2 , 2.66×10 2 )Toluene (Mw = 92)
[0221] (7) Sample: 0.05 g sample in 10 mL THF solution
[0222] ·Measurement method
[0223] First, polystyrene was used as a standard substance, and a calibration curve was obtained based on a graph detected by a refractive index difference. Next, for each sample, based on the same calibration curve, the mass % of the peak near the peak top molecular weight (number average molecular weight) of MDI of 250 was obtained based on a graph detected by a refractive index difference.
[0224] <Determination of NCO content>
[0225] The NCO content was measured in accordance with JIS K1603-1:2007.
[0226] <Preparation Examples B-1 to B-6>
[0227] The raw materials shown in Table 5 were added at the composition ratios shown in Table 5, stirred and uniformly mixed, to obtain polyols B-1 to B-6.
[0228] [Table 5]
[0229]
[0230] <Examples 1 to 9, Comparative Examples 1 to 6>
[0231] The polyisocyanate composition (main agent) and the polyol (curing agent) were mixed in the compositions shown in Tables 6, 7 and 8 to prepare polyurethane resin-forming compositions, which were evaluated by the following method.
[0232] <Mixed viscosity and pot life test>
[0233] The main agent and the curing agent, which were previously adjusted to a temperature of 45° C., were measured and mixed in a total of 50 g in a formulation of isocyanate group / hydroxyl group=1.00 to 1.05 (molar ratio) to obtain a mixture.
[0234] Next, the viscosity of the mixture was measured at 25°C using a rotational viscometer (type B, rotor No. 4). The viscosity was determined 60 seconds after the main agent and curing agent were mixed and was taken as the mixed viscosity. In addition, the time until the viscosity of the mixture reached 50,000 mPa·s was determined and taken as the pot life (seconds).
[0235] If the mixed viscosity is 1900 mPa·s or less, the filling property is judged to be good. If the pot life is within 300 seconds, the rapid curing property is judged to be good.
[0236] <Hardness (10 seconds value)>
[0237] Adjust the main agent and curing agent to 45°C respectively, quickly measure 60g of the main agent in a 500ml plastic cup (Polycup), and then quickly measure 40g of the curing agent. Mix with a spatula for 30 seconds and perform vacuum degassing at 50mmHg for 60 seconds. After degassing, transfer 80g to a 300ml plastic cup and mature at 45°C for 48 hours. Take out the cured product from the plastic cup, place it at 25°C for 4 hours, and measure the hardness using a Durometer D hardness meter. Press the hardness meter and calculate the reading value after 10 seconds as the hardness (10 second value).
[0238] <Determination of low molecular weight dissolution value>
[0239] Preparation of test samples
[0240] The main agent and the curing agent were mixed at a liquid temperature of 45° C. so that the isocyanate group / hydroxyl group ratio was 1.00 to 1.05 (molar ratio) and the total mass was 30 g to obtain a mixed liquid.
[0241] The obtained mixed solution was stirred for 15 seconds, and 10 g of glycerol (assumed to be glycerol contained in the hollow fiber) was further added and stirred for 15 seconds to obtain a composition. The composition was allowed to stand in a thermostatic bath under the conditions of a temperature of 50° C. and a time of 10 minutes as the primary curing condition, and allowed to stand in a thermostatic bath under the conditions of a temperature of 45° C. and a time of 2 days as the secondary curing condition to obtain a test sample.
[0242] Determination of low molecular weight dissolution value
[0243] Cut the test sample into a fan shape and weigh 20g, immerse it in 100mL purified water preheated to 40°C, place it at 40°C for 2 hours, and extract the low-molecular-weight dissolved matter in the purified water. Next, decant the obtained extract, pour 10ml into a 50ml volumetric flask, and use purified water to make 50ml of the liquid as the test solution. Then, perform UV absorbance measurement of the test solution (manufactured by Shimadzu Corporation, product name UV-1500). One tenth of the maximum value of the absorbance at 240 to 245nm is taken as the low-molecular-weight dissolved matter value. If the low-molecular-weight dissolved matter value is less than 0.05, it can be judged that there is little dissolved matter.
[0244] <Evaluation of whiteness>
[0245] Preparation of samples for whiteness evaluation
[0246] A sample for whiteness evaluation was obtained by the same method as in <Hardness (10 seconds value)>.
[0247] Evaluation of whiteness
[0248] The whiteness of the obtained whiteness evaluation sample is measured. The whiteness is measured in accordance with JIS-P8123. The whiteness is preferably 10 or less, more preferably 8 or less.
[0249] [Table 6]
[0250] Example 1 Example 2 Example 3 Example 4 Example 5 Main agent A-1 A-2 A-3 A-4 A-5 Curing agent B-1 B-2 B-3 B-2 B-2 NCO / OH (molar ratio) 1.01 1.00 1.03 1.00 1.00 Cross-linking group density (mmol / g) 0.92 0.95 0.95 0.95 0.94 Mixed viscosity (mPa·s) 1350 1860 1730 1700 1600 Applicable period (seconds) 500 200 207 198 215 hardness 64 55 56 55 55 Low molecular weight dissolution value 0.049 0.048 0.044 0.049 0.048 Whiteness 6.3 8.4 7.6 7.1 6.8
[0251] [Table 7]
[0252] Example 6 Example 7 Example 8 Example 9 Main agent A-6 A-3 A-3 A-7 Curing agent B-3 B-5 B-6 B-1 NcO / oH (molar ratio) 1.03 1.04 1.00 1.01 Cross-linking group density (mmol / g) 095 090 0.90 092 Mixed viscosity (mPa·s) 1850 1600 1530 1320 Applicable period (seconds) 200 200 205 530 hardness 57 54 54 64 Low molecular weight dissolution value 0.049 0042 0.048 0.050 Whiteness 7.0 7.5 7.0 6.3
[0253] [Table 8]
[0254] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Main agent A’-1 A’-2 A’-3 A’-4 A’-5 A’-6 Curing agent B-2 B-2 B-2 B-2 B-3 B-4 NCO / OH (molar ratio) 100 100 100 100 103 102 Cross-linking group density (mmol / g) 095 095 095 097 095 065 Mixed viscosity (mPa·s) 1980 1800 1270 1650 2040 200 Applicable period (seconds) 191 197 219 213 197 2880 hardness 54 54 54 56 58 30 Low molecular weight dissolution value 0.038 0.044 0.059 0.060 0.054 0.18 Whiteness 48 18.6 6.0 6.3 6.8 5.9
[0255] Description of Reference Numerals
[0256] 11 Shell
[0257] 13Hollow fiber membrane
[0258] 151st fluid inlet
[0259] 171st fluid outlet
[0260] 19 membrane sealing material
[0261] 100 membrane modules (hollow fiber membrane modules)
Claims
1. A polyisocyanate composition comprising a polyisocyanate (A), The polyisocyanate (A) comprises: Diphenylmethane diisocyanate (a1), Isocyanate-terminated prepolymer (a2), and Isocyanate-modified product (a3), The isocyanate-terminated prepolymer (a2) is a reaction product of a polyisocyanate (a2-1) and a polyol (a2-2). The polyisocyanate (a2-1) comprises diphenylmethane diisocyanate (a2-1-1) and a modified isocyanate (a2-1-2), The modified isocyanate (a2-1-2) is at least one selected from the group consisting of carbodiimide-modified diphenylmethane diisocyanate and uretonimine-modified diphenylmethane diisocyanate, The modified isocyanate (a3) is a modified diphenylmethane diisocyanate. The content of the modified isocyanate (a2-1-2) in the polyisocyanate (a2-1) is 4.5 to 15% by mass.
2. The polyisocyanate composition according to claim 1, wherein The modified isocyanate (a3) includes at least one selected from the group consisting of carbodiimide-modified diphenylmethane diisocyanate and uretonimine-modified diphenylmethane diisocyanate.
3. The polyisocyanate composition according to claim 1, wherein In the polyisocyanate (A), the total content of the structural unit derived from the modified isocyanate (a2-1-2) and the modified isocyanate (a3) is 4.5 to 15% by mass.
4. The polyisocyanate composition according to claim 1, wherein In the isocyanate-terminated prepolymer (a2), the content ratio of the structural unit derived from 4,4′-diphenylmethane diisocyanate in the structural unit derived from diphenylmethane diisocyanate is 50 to 80%.
5. The polyisocyanate composition according to claim 1, wherein In the isocyanate-terminated prepolymer (a2), the total content ratio of the structural unit derived from 2,2′-diphenylmethane diisocyanate and the structural unit derived from 2,4′-diphenylmethane diisocyanate in the structural unit derived from diphenylmethane diisocyanate is 20 to 50%.
6. A polyurethane resin-forming composition comprising: The polyisocyanate composition according to any one of claims 1 to 5, and Polyol (B).
7. The polyurethane resin-forming composition according to claim 6, wherein The polyol (B) comprises: At least one polyol (b1) selected from the group consisting of castor oil, partially dehydrated castor oil and castor oil-modified polyol; and An amine compound (b2) having two or more hydroxyl groups.
8. The polyurethane resin-forming composition according to claim 7, wherein The content of the amine compound (b2) in the polyol (B) is 30% by mass or less. 9 . The polyurethane resin-forming composition according to claim 6 , which has a crosslinking group density of 0.9 mmol / g or more.
10. The polyurethane resin-forming composition according to claim 6, which is used for a film sealing material. 11 . A film sealing material comprising a cured product of the polyurethane resin-forming composition according to claim 10 .
12. A membrane module comprising: Main body, Membranes, and a membrane sealing material for sealing a gap between the main body and the membrane, The film sealing material is the film sealing material according to claim 11.
13. The membrane module according to claim 12, wherein: The membrane comprises a plurality of hollow fiber membranes, The membrane sealing material seals a gap between the main body and at least a part of the hollow fiber membranes and at least a part of a gap between the hollow fiber membranes.