Method for manufacturing wafer using release tape and adhesive material, and release tape and adhesive material used in said method

By using the release tape and bonding material of silicone-based adhesive components with a specific peel strength ratio, the problem of difficulty in removing bonding materials in wafers is solved, and an efficient and stable removal process is achieved, which improves the wafer's Productivity and pass rate.

CN118946952APending Publication Date: 2024-11-12MITSUI CHEM ICT MATERIA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094351.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-11-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art tends to remain residual glue when removing bonded materials from wafers, affecting the passing rate and production efficiency of wafers.

Method used

Using the release tape and bonding material of silicone-based adhesive component with a specific peel strength ratio, the adhesive force between the peel tape and the bonding material and the bonding force between the wafer can be achieved by adjusting the adhesive force between the peel tape and the bonding material. and simple bonding material removal.

Benefits of technology

It effectively avoids residual glue residues of bonded materials, improves wafer productivity and pass rate, and improves the production efficiency of semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946952A_ABST
    Figure CN118946952A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a method for manufacturing a wafer by which an adhesive material can be easily and stably peeled off from a laminate comprising a wafer and the adhesive material compared to a known method. In addition, the present invention addresses the problem of providing an adhesive material and a release tape which can be easily and stably peeled compared to the known adhesive material. The problem of the present invention is solved by a method for manufacturing a wafer, the method including a step of peeling an adhesive material from a laminate (A) comprising a wafer and the adhesive material using a peeling tape, the peeling tape used in the previous step contains a silicone adhesive component in an adhesive layer in contact with the adhesive material, and the adhesive material used in the previous step has P1 and P2 satisfying the peel strength ratio P1 / P2 of 6 or more and P2 of 0.5 N / 25 mm or more; wherein the adhesive bonding material has a surface A in contact with the release tape and a surface B in contact with the wafer, P1 is the peel strength of the surface A when measured such that the release tape is held at 90 DEG with respect to the adhesive bonding material, and P2 is the peel strength of the surface B when measured such that the adhesive bonding material is held at 90 DEG with respect to the polyimide-coated wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a wafer, and more specifically, to a method for manufacturing a wafer comprising the following steps: after processing a wafer such as a wafer temporarily fixed to a support, using a peeling tape to peel off an adhesive material temporarily fixing the wafer to the support from the wafer. Background Art

[0002] In the semiconductor manufacturing process, when handling wafers, it is often necessary or desirable to temporarily fix the wafers due to reasons such as wafer thinning or easy breakage. For example, in order to achieve high integration of semiconductor devices, thin grinding and cutting of wafers with functional layers for semiconductor devices has been widely performed. However, if the wafers are ground and cut to extremely thin thickness, it is impossible to support the wafers only with tape. Therefore, a method of temporarily fixing the wafers to a hard carrier (support body) through an adhesive material and performing the treatment after thin grinding and cutting is proposed. The semiconductor manufacturing process using such a support body is called a wafer support system.

[0003] In a wafer manufacturing process using a wafer support system, after a wafer thinning process or the like, the support body is peeled off from the wafer, and thereafter, the adhesive material temporarily fixing the wafer and the support body must be removed from the wafer.

[0004] As a method for removing adhesive bonding materials, a method is known in which a peeling tape is attached and then peeled off so that unnecessary materials on a semiconductor wafer are peeled off together with the peeling tape (Patent Document 1). In addition, a method for removing a temporary fixing material by an adhesive sheet (bonding tape) that can be easily removed from a wafer and an adhesive sheet thereof have been proposed (Patent Documents 2 and 3).

[0005] In addition, a bonding agent that can be removed from a wafer more easily has been proposed (Patent Document 4).

[0006] However, when using these peeling tapes or adhesive tapes, or bonding agents, it is not easy to peel them off from the end of the bonding material. When peeling the bonding material, sometimes a part of the bonding material remains on the wafer, which is called residual adhesive, and affects the yield of the wafer.

[0007] [Prior art literature]

[0008] [Patent Document]

[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 2002-124494

[0010] [Patent Document 2] Japanese Patent Application Publication No. 2009-275060

[0011] [Patent Document 3] Japanese Patent Publication No. 2015-518270

[0012] [Patent Document 4] International Publication No. 2017 / 221772A1. Summary of the invention

[0013] [Problems to be solved by the invention]

[0014] In view of the above-mentioned prior art, an object of the present invention is to provide a method for manufacturing a wafer, which includes: using a peeling tape to peel off an adhesive material from a stacked body A consisting of a wafer and an adhesive material, and compared with the known peeling method, the adhesive material can be peeled off from the stacked body A consisting of a wafer and an adhesive material more simply and stably. In addition, another object of the present invention is to provide an adhesive material and a peeling tape that can be peeled off more simply and stably than the known ones.

[0015] [Methods to solve the problem]

[0016] The adhesive material can be used in a wafer processing method (wafer support system) in which the wafer is temporarily fixed to a support body for grinding, cutting and other processing. The adhesive material has surfaces A and B. In order to temporarily fix the support body and the wafer, surface A is attached to the support body and surface B is attached to the side of the wafer, and is used for processing the wafer.

[0017] After the wafer is processed, the support is removed, and a laminated body A composed of the wafer and the adhesive material can be obtained. The present invention relates to a method for removing the adhesive material from the laminated body A.

[0018] The adhesive material may include an adhesive layer with face A and an adhesive layer with face B, and may preferably include a release tape side adhesive layer, a substrate film, and a wafer side adhesive layer. In addition, the adhesive material may be a single-layer adhesive layer formed by hardening a semi-liquid or liquid adhesive. At this time, there is a release tape side adhesive layer and a wafer side adhesive layer made of the same material.

[0019] As a result of diligent research, the inventors discovered that by using a peeling tape and an adhesive material whose peel strength between the peeling tape / adhesive material and the peel strength between the adhesive material and a specific wafer satisfy specific conditions, the adhesive material can be stably peeled off from the stack A composed of the wafer and the adhesive material relatively easily, thereby completing the present invention.

[0020] That is, the present invention and its various aspects are as follows. However, the present invention is not limited to the following. [1]

[0022] A method for manufacturing a wafer, comprising:

[0023] The step of peeling the adhesive material from the laminate A consisting of the wafer and the adhesive material using a peeling tape,

[0024] The release tape used in the above step contains a silicone adhesive component in the adhesive layer in contact with the above adhesive material.

[0025] The adhesive materials used in the above steps have P1 and P2 that satisfy a peel strength ratio P1 / P2 of 6 or more and P2 of 0.5N / 25mm or more;

[0026] Among them, the above-mentioned adhesive material has a surface A connected to the above-mentioned release tape and a surface B connected to the wafer, P1 is the peel strength of surface A when the above-mentioned release tape is measured at 90° relative to the above-mentioned adhesive material, and P2 is the peel strength of surface B when the above-mentioned adhesive material is measured at 90° relative to the polyimide coated wafer. [2]

[0028] The wafer manufacturing method according to [1], wherein the layer having the surface A of the adhesive material contains a silicone-based adhesive component or a silicone release agent. [3]

[0030] The wafer manufacturing method according to [1] or [2], wherein the adhesive material has at least a wafer-side adhesive layer, a base film, and a release tape-side adhesive layer. [4]

[0032] A peeling method, which uses a peeling tape to peel off the adhesive material from a laminated body A consisting of a wafer and an adhesive material,

[0033] The release tape used in the release method contains a silicone adhesive component in the adhesive layer in contact with the adhesive material.

[0034] The adhesive material used in the peeling method has P1 and P2 satisfying a peel strength ratio P1 / P2 of 6 or more and P2 of 0.5 N / 25 mm or more;

[0035] Among them, the above-mentioned adhesive material has a surface A connected to the above-mentioned release tape and a surface B connected to the wafer, P1 is the peel strength of surface A when the above-mentioned release tape is measured at 90° relative to the above-mentioned adhesive material, and P2 is the peel strength of surface B when the above-mentioned adhesive material is measured at 90° relative to the polyimide coated wafer. [5]

[0037] The peeling method according to [4], wherein the layer having the surface A of the adhesive material contains a silicone-based adhesive component or a silicone release agent. [6]

[0039] The peeling method according to [4] or [5], wherein the adhesive material has at least a wafer-side adhesive layer, a base film, and a peeling tape-side adhesive layer. [7]

[0041] An adhesive material used in the wafer manufacturing method or the wafer peeling method according to any one of [1] to [6], wherein P2 is 0.5 N / 25 mm or more. [8]

[0043] A release tape used in the wafer manufacturing method or release method described in any one of [1] to [6], wherein the release tape comprises at least a base film and an adhesive layer, and the adhesive layer contains a silicone-based adhesive. [9]

[0045] The release tape according to claim 8, wherein the base film of the release tape comprises at least one of polyimide, polyester, or fluororesin.

[0046] [Effects of the invention]

[0047] If the wafer manufacturing method of the present invention is used, the adhesive material can be simply and stably removed from the wafer after the wafer has been processed by thin grinding and cutting, so no residual glue or damage to the wafer will be generated, and it can be implemented with high productivity and pass rate, which greatly contributes to the improvement of the productivity of electronic parts such as electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Part (a) of Fig. 1 is a schematic diagram for explaining a method for measuring the peel strength P1 using a test sample for measuring the peel strength P1. The composition of the peel strength P1 of the wafer side adhesive layer that does not contribute to the adhesive material is omitted, and the ratios between the sizes of the components in the figure do not reflect the actual ratios.

[0049] Part (b) of Fig. 1 is a schematic diagram for explaining a method for measuring the peel strength P2 using a test specimen for measuring the peel strength P2. The composition of the peel strength P2 of the peeling tape side bonding layer that does not contribute to the bonding material is omitted, and the ratios between the sizes of the components in the figure do not reflect the actual ratios.

[0050] Figure 2 This is a schematic diagram showing a laminate composed of release tape / adhesive material / wafer when a double-sided tape having a base film as an adhesive material is used. The ratios between the dimensions of the components in the figure do not reflect the actual ratios.

[0051] Figure 3The present invention is a schematic diagram showing a method for removing a support from a stacked body B composed of a support / adhesive material / wafer to produce a stacked body A composed of a wafer and an adhesive material in a method for evaluating removability from a wafer. However, from the perspective of simplification, the adhesive material is illustrated as a single-layer structure, and the ratios between the sizes of the components in the figure do not reflect the actual ratios.

[0052] Figure 4 This is a schematic diagram showing a method for evaluating the removability from a wafer. For the sake of simplicity, the adhesive material is shown as a single-layer structure, and the ratios between the dimensions of the components in the figure do not reflect the actual ratios. DETAILED DESCRIPTION

[0053] The method for manufacturing a wafer of the present invention comprises:

[0054] The step of peeling the adhesive material from the laminate A consisting of the wafer and the adhesive material using a peeling tape,

[0055] The release tape used in the above step contains a silicone adhesive in the adhesive layer in contact with the above adhesive material.

[0056] The adhesive materials used in the above steps have P1 and P2 that satisfy a peel strength ratio P1 / P2 of 6 or more and P2 of 0.5N / 25mm or more;

[0057] Among them, the above-mentioned adhesive material has a surface A connected to the above-mentioned release tape and a surface B connected to the wafer, P1 is the peel strength of surface A when the above-mentioned release tape is measured at 90° relative to the above-mentioned adhesive material, and P2 is the peel strength of surface B when the above-mentioned adhesive material is measured at 90° relative to the polyimide coated wafer.

[0058] That is, in the wafer manufacturing method of the present invention, an adhesive material and a release tape are used.

[0059] Bonding materials

[0060] The adhesive material used in the wafer manufacturing method of the present invention has P1 and P2 that satisfy the peel strength ratio P1 / P2 of 6 or more, and P2 of 0.5N / 25mm or more. Wherein, the aforementioned adhesive material has a surface A in contact with the aforementioned peeling tape, and a surface B in contact with the wafer, P1 is the peel strength of surface A when the aforementioned peeling tape is held at 90° relative to the aforementioned adhesive material, and P2 is the peel strength of surface B when the aforementioned adhesive material is held at 90° relative to the polyimide coated wafer.

[0061] The peel strength P1 is the adhesive strength on the surface A (that is, between the peel tape and the adhesive material), and the peel strength P2 is the adhesive strength on the surface B (that is, between the adhesive material and the wafer). In the evaluation of the peel strength P2, the peel strength between the adhesive material and the polyimide coated wafer is measured by using a polyimide coated wafer as a wafer for peel strength measurement.

[0062] The peel strength P1 and peel strength P2 of the adhesive used in the present invention are the force (N / mm) per unit width of the peeled portion required to peel while maintaining the angle between the peeled layers (peel tape and adhesive, or adhesive and wafer) at 90°.

[0063] That is, the peel strength P1 and the peel strength P2 are measured by peeling the adhesive tape / adhesive material or the adhesive material / wafer in the state shown in FIG1 or in a state based thereon, and the force required for peeling is measured. The measured value can be determined by dividing the width of the peeled portion, and more specifically, the measurement can be performed according to the following method.

[0064] When measuring the peel strength P1 between the release tape and the adhesive material, the measurement can be performed using a sample for measuring the peel strength P1 without a wafer (part (a) of FIG. 1 ).

[0065] The sample for measuring the peel strength P1 is obtained, for example, by fixing the wafer side adhesive layer of the adhesive material to an acrylic plate (not shown) via a double-sided tape. Before the adhesive material is fixed to the acrylic plate, the actual wafer manufacturing steps can be preset, and treatments such as heating can be performed. After the adhesive layer 22 of the peeling tape side adhesive layer 22 of the adhesive material of the obtained sample for measuring the peel strength P1 is attached to the adhesive layer 22 of the peeling tape by a predetermined method, the peeling tape can be peeled off while keeping the angle formed by the peeling tape and the adhesive material at 90° to measure the peel strength P1 (part (a) of Figure 1).

[0066] When measuring the peel strength P2 between the adhesive material and the wafer, the peel strength P2 measurement sample without the peeling tape can be used for measurement (part (b) of FIG. 1 ).

[0067] The peel strength P2 measurement sample can be obtained, for example, by attaching the wafer side adhesive layer 23 of the adhesive material to the polyimide coated wafer 3 for measurement. At this time, the actual wafer manufacturing steps can be preset, and treatments such as heating can be performed. From the obtained peel strength P2 measurement sample, the adhesive material can be peeled off while keeping the adhesive material and the angle formed at 90°, and the peel strength P2 can be measured (part (b) of Figure 1).

[0068] The peel strength ratio P1 / P2 is 6 or more, preferably 6.5 or more.

[0069] There is no upper limit in particular in the above-mentioned peel strength ratio P1 / P2, but the above-mentioned peel strength ratio P1 / P2 is preferably less than 30, more preferably less than 25, and particularly preferably less than 20. From the viewpoint that the laminated body A consisting of wafer and adhesive material properly peels off the adhesive material, it is hoped that the peel strength P2 between the adhesive material / wafer should not be too large, and from the viewpoint of preventing the unexpected peeling and residual adhesive of the peeling tape and the adhesive material, it is hoped that the peel strength P1 between the peeling tape / adhesive material should not be too small. By having a peel strength ratio P1 / P2 of more than 6, the unexpected peeling of the peeling tape and the adhesive material and the residual adhesive on the wafer can be prevented.

[0070] The peel strength P1 is not particularly limited as long as it satisfies the above-mentioned peel strength ratio P1 / P2, but is preferably 3N / 25mm or more. The peel strength P1 is more preferably 5N / 25mm or more, and particularly preferably 8N / 25mm or more. In addition, the peel strength P1 is not particularly limited as long as it satisfies the above-mentioned peel strength ratio P1 / P2, but is preferably 60N / 25mm or less. The peel strength P1 is more preferably 30N / 25mm or less, and particularly preferably 20N / 25mm or less.

[0071] When the peel strength P1 is 3 N / 25 mm or more, when the adhesive is peeled off from the laminate A consisting of the wafer and the adhesive, unexpected peeling of the peeling tape and the adhesive and adhesive residue on the wafer can be prevented.

[0072] The peel strength P2 is 0.5 N / 25 mm or more. The peel strength P2 is preferably 0.7 N / 25 mm or more.

[0073] The upper limit of the peel strength P2 is not particularly limited as long as the above-mentioned peel strength ratio P1 / P2 is satisfied, but is preferably 2.5 N / 25 mm or less, and more preferably 2 N / 25 mm or less.

[0074] When the peel strength P2 is 0.5N / 25mm or more, the wafer can be prevented from peeling off from the support during the wafer thin grinding and cutting process. When the peel strength P2 is 2.5N / 25mm or less, when the adhesive material is peeled off from the wafer, the unexpected peeling of the peeling tape and the temporary fixing material and the residual adhesive on the wafer can be prevented.

[0075] The above-mentioned method for adjusting the peel strength P1, peel strength P2, and peel strength ratio P1 / P2 is not particularly limited, but for example, it can be appropriately increased or decreased by the method used in the past in this technical field. More specifically, it can be appropriately increased or decreased by the composition or manufacturing process of each layer described later, the manufacturing process of the laminate B composed of the support / adhesive material / wafer, etc. For example, by: using a polymer with high polarity for the adhesive material; adding a tackifying resin such as polybutene, rosin resin, terpene resin, petroleum resin, coumarin resin, etc.; or reducing the cross-linking component, etc.; the peel strength P1 and / or the peel strength P2 can be increased. On the other hand, for example, by: adding a release agent to the adhesive material; increasing the cross-linking component; or using a polymer with low polarity, etc.; the peel strength P1 and / or the peel strength P2 can be reduced.

[0076] The adhesive material used in the wafer manufacturing method of the present invention may have a single-layer structure or a multi-layer stacked structure.

[0077] When the adhesive material is a single-layer structure, the whole of the adhesive material can have the same composition, for example, can be the adhesive tape of the monolayer comprising the adhesive composition. In addition, the adhesive material can use semi-liquid or liquid hardening type adhesive as the precursor of the adhesive material. When using semi-liquid or liquid hardening type adhesive, make the semi-liquid or liquid adhesive be coated on any one of a support or wafer or both thereof, after spin coating, by making the support and wafer fit across the adhesive, and the adhesive composition is hardened, the laminated body B consisting of support / adhesive material / wafer can be made. After removing the support from laminated body B, the face connected with the support of the adhesive becomes the face A connected with the stripping tape.

[0078] When the adhesive material is a multi-layer laminated structure, the adhesive material may include: a layer having a surface A in contact with the release tape and a layer having a surface B in contact with the wafer having different compositions. In this case, the layer having surface A and the layer having surface B may be a layered structure in the general sense in which the composition at the interface changes discontinuously, but may also be a structure having a so-called inclined composition in which the composition changes continuously.

[0079] In addition, when the adhesive material is a multi-layer laminated structure, it can be a so-called double-sided tape in which both the layer having surface A and the layer having surface B are adhesive layers. In this case, the layer having surface A can be configured in a manner to have a predetermined peel strength between the release tape and the adhesive material, and the layer having surface B can be configured in a manner to have a predetermined peel strength between the adhesive material and the wafer.

[0080] The layer having surface A is in contact with the support body in the wafer support system in order to temporarily fix the wafer, so it can be formed by considering the bonding strength between the adhesive material and the support body. For example, when a semi-liquid or liquid adhesive is used to bond the support body and the wafer, and then the adhesive component is hardened to form a laminated body B consisting of the support body / adhesive material / wafer, the layer having surface A of the adhesive material can contain a hardening adhesive component.

[0081] The adhesive composition used in the adhesive layer of the adhesive material can be, for example, rubber, acrylic, epoxy, urethane, allyl, silicone, fluorine, and polyimide adhesive compositions. Because it has heat resistance and is easy to adjust the adhesive strength, acrylic or silicone adhesive compositions are preferred. In particular, from the viewpoint of adjusting the adhesive strength with the release tape, when the layer with face A of the aforementioned adhesive material is an adhesive layer, the adhesive layer preferably contains an acrylic adhesive composition containing a silicone release agent.

[0082] The adhesive component may be a hardening adhesive component or a non-hardening adhesive component. By hardening it before heat treatment, it is difficult to generate holes during the heat treatment in the manufacturing step, and the bonding deterioration caused by the high temperature during the heat treatment can be suppressed, so that it is easy to peel off without residual adhesive, so the hardening adhesive component is preferred.

[0083] Examples of the curable adhesive component include a photocurable adhesive component that is cross-linked and cured by light irradiation and a thermocurable adhesive component that is cross-linked and cured by heating.

[0084] The above-mentioned photocuring adhesive component or thermosetting adhesive component can be, for example, a monomer, oligomer or polymer containing acrylic acid, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate as a curing component, and a photocuring adhesive component or thermosetting adhesive component containing a photopolymerization initiator or a thermopolymerization initiator.

[0085] Among the above, the polymer of the acrylic adhesive component can be obtained by, for example, pre-synthesizing a (meth)acrylic polymer having a functional group in the molecule (hereinafter referred to as a (meth)acrylic polymer containing a functional group), and reacting it with a compound having a functional group reactive with the above functional group and a free radical polymerizable unsaturated bond in the molecule (hereinafter referred to as an unsaturated compound containing a functional group).

[0086] The (meth) acrylic polymer containing a functional group is obtained by copolymerizing an alkyl acrylate and / or alkyl methacrylate having an alkyl group carbon number of usually 2 to 18 as a main monomer with a monomer containing a functional group and other monomers for modification which can be copolymerized with these monomers as needed according to a common method. The weight average molecular weight of the (meth) acrylic polymer containing a functional group is usually about 200,000 to 2,000,000.

[0087] Examples of the functional group-containing monomer include carboxyl-containing monomers such as acrylic acid and methacrylic acid, hydroxyl-containing monomers such as hydroxyethyl acrylate and hydroxyethyl methacrylate, epoxy-containing monomers such as glycidyl acrylate and glycidyl methacrylate, isocyanate-containing monomers such as isocyanateethyl acrylate and isocyanateethyl methacrylate, and amine-containing monomers such as aminoethyl acrylate and aminoethyl methacrylate.

[0088] Examples of the other copolymerizable modifying monomers include various monomers used in general (meth)acrylic polymers such as vinyl acetate, acrylonitrile, and styrene.

[0089] The unsaturated compound containing a functional group that reacts with the above-mentioned (meth) acrylic polymer containing a functional group may be the same compound as the above-mentioned monomer containing a functional group, depending on the functional group of the above-mentioned (meth) acrylic polymer containing a functional group. For example, when the functional group of the above-mentioned (meth) acrylic polymer containing a functional group is a carboxyl group, an epoxy group-containing monomer or an isocyanate group-containing monomer is used. When the functional group of the above-mentioned (meth) acrylic polymer containing a functional group is a hydroxyl group, an isocyanate group-containing monomer is used. When the functional group of the above-mentioned (meth) acrylic polymer containing a functional group is an epoxy group, a carboxyl group-containing monomer or an amide group-containing monomer such as acrylamide is used. When the functional group of the above-mentioned (meth) acrylic polymer containing a functional group is an amine group, an epoxy group-containing monomer is used.

[0090] The above-mentioned photopolymerization initiator can be, for example, a photopolymerization initiator activated by irradiating light of a wavelength of 250 to 800 nm. Such a photopolymerization initiator can be, for example, an acetophenone derivative compound such as methoxyacetophenone, or a benzoin ether-based compound such as benzoin propyl ether and benzoin isobutyl ether, or a ketal derivative compound such as benzyl dimethyl ketal and acetophenone diethyl ketal, or a phosphine oxide derivative compound, or a bis(η5-cyclopentadienyl) titanocene derivative compound, benzophenone, Michler's ketone, chlorothioxanthone, dodecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexyl phenyl ketone, 2-hydroxymethylphenylpropane, etc. Photoradical polymerization initiators. These photopolymerization initiators can be used alone or in combination of two or more.

[0091] The above-mentioned thermal polymerization initiator can be a thermal polymerization initiator that decomposes by heat and generates active free radicals that start polymerization and curing. Specifically, for example, tert-butyl peroxy-2-ethylhexanoate, bis(4-methylbenzoyl) peroxide, benzoyl peroxide, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(4,4-bis-(tert-butylperoxy)cyclohexyl)propane, tert-hexyl peroxyisopropyl monocarboxylate, tert-butyl peroxyacetate, 2,2-bis-(tert-butylperoxy)cyclohexane, 4,4-bis-(tert-butylperoxy)pentanoic acid n-butyl ester, di-tert-hexyl peroxide, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, bis(2-tert-butylperoxyisopropyl)benzene, tert-butylisopropylbenzene peroxide, di-tert-butyl 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne, diisopropylbenzene hydroperoxide, etc.

[0092] Among these thermal polymerization initiators, commercially available thermal polymerization initiators are not particularly limited, but suitable examples include PERBUTYL O, NYPER BMT, NYPER BW, PERHEXA HC, PERHEXA C, PERTETRA A, PERHEXYL I, PERBUTYL A, PERHEXA 22, PERHEXA V, PERHEXYL D, PERCUMYL D, PERHEXA 25B, PERBUTYL P, PERBUTYL C, PERHEXYNE 25B, PERCUMYL P (all of which are manufactured by NOF Corporation), PERKADOX 12XL25 (manufactured by Kayaku NOURYON Co., Ltd.), etc. These thermal polymerization initiators may be used alone or in combination of two or more.

[0093] The oligomer or monomer as the curing component generally has a molecular weight of 10,000 or less, and the number of radically polymerizable unsaturated bonds in the molecule is 1 to 40. From the viewpoint of three-dimensional network formation, the number of radically polymerizable unsaturated bonds is preferably 2 or more.

[0094] Examples of oligomers or monomers as the curing component include trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxy pentaacrylate, dipentaerythritol hexaacrylate, or the same methacrylates as above. Other examples include 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, commercially available oligoester acrylates, urethane acrylates, and the same methacrylates as above. These multifunctional oligomers or monomers may be used alone or in combination of two or more.

[0095] The adhesive material may contain, as desired, acrylic polymers without unsaturated double bonds, or various thermal crosslinking agents such as isocyanate compounds, melamine compounds, and epoxy compounds, or publicly known additives such as release agents, plasticizers, resins, surfactants, waxes, and microparticle fillers.

[0096] In the adhesive material, a release agent can be preferably used from the viewpoint of adjusting the peel strength between the release tape / adhesive material and / or between the adhesive material / wafer.

[0097] The release agent is generally not particularly limited as long as it can exert a release effect, and examples thereof include hydrocarbon compounds, silicone compounds, fluorine compounds, polyethylene wax, carnauba wax, montanic acid, stearic acid, etc., which are known as release agents for plastic materials.

[0098] In addition, other release agents include plasticizers. The plasticizer is generally not particularly limited as long as it reduces the adhesive strength of the adhesive material to the adherend. For example, plasticizers such as trimellitic acid esters, pyromellitic acid esters, phthalic acid esters, and adipic acid esters can be listed.

[0099] The release agent is preferably a silicone-based or fluorine-based compound, and more preferably a silicone-based or fluorine-based compound having a functional group that can cross-link with the curable adhesive.

[0100] In particular, the silicone compound contained in the silicone release agent has excellent heat resistance, so even after being treated with heating at more than 200°C, it can prevent the adhesive from being burned, etc., and it can easily be peeled off because it seeps out to the interface of the adherend during peeling. Since the silicone compound has a functional group that can cross-link with the above-mentioned curable adhesive, it will chemically react with the above-mentioned curable adhesive due to light irradiation or heating and be introduced into the above-mentioned curable adhesive, so the silicone compound will not adhere to the adherend and cause contamination. In addition, by formulating the silicone compound, it also has the effect of preventing residual glue on the semiconductor chip.

[0101] In one aspect of the present invention, the layer having the surface A of the adhesive material may contain a silicone release agent.

[0102] The addition amount of the release agent is not particularly limited, but can be suitable for determining the addition amount that can obtain the release effect. On the other hand, in order to avoid significantly damaging the bonding function of the bonding material, the addition amount is controlled to be not excessive. For example, relative to 100 mass parts of the bonding material as a whole, usually with 0.1 to 5 mass parts, preferably 0.1 to 3 mass parts, more preferably 0.1 to 1 mass part or so addition amount as a target, it is desired to adjust according to the peeling force.

[0103] When a plasticizer is added, the target amount is usually 5 to 50 parts by mass, preferably 10 to 50 parts by mass, and more preferably 20 to 40 parts by mass, and it is desirable to adjust the amount according to the peeling force.

[0104] In this aspect, these release agents may be used alone or in combination of two or more.

[0105] In one embodiment, the layer having surface A of the adhesive material may contain a silicone adhesive component or a silicone release agent. By containing a silicone adhesive component or a silicone release agent in the layer having surface A, the peeling tape is adhered to the end of the adhesive material, and it is easy to create a start when peeling the adhesive material from the wafer, so that the adhesive material can be more easily peeled from the laminate A composed of the wafer and the adhesive material.

[0106] The thickness of the adhesive material is not particularly limited, but the preferred lower limit is 5 μm, the preferred upper limit is 250 μm, the more preferred lower limit of the thickness of the adhesive material is 10 μm, and the more preferred upper limit is 200 μm. If the thickness of the adhesive material is within this range, the concavo-convex of the wafer can be absorbed and temporarily fixed to the support with sufficient strength, and the peeling force can be easily adjusted to a suitable range when peeling the adhesive material.

[0107] In one embodiment, the adhesive material used in the manufacture method of wafer of the present invention preferably has a substrate film between the stripping tape side adhesive layer and the wafer side adhesive layer, namely the so-called double-sided adhesive tape. In this state, the aforementioned stripping tape side adhesive layer and the aforementioned wafer side adhesive layer can be designed from the viewpoint of making the peel strength between the stripping tape / adhesive material and / or the adhesive material / wafer as the optimum strength. Due to the viewpoint of the mechanical strength or operability of the laminated body B constituted by the support / adhesive material / wafer when the adhesive material itself or the temporarily fixed support and the wafer, the substrate film is designed, so from the viewpoint of making the performance of the adhesive material as the optimum, it is particularly advantageous.

[0108] At Figure 2 1 shows an example of a laminate composed of a release tape / adhesive material / wafer when a double-sided tape having a base film between the wafer-side adhesive layer and the release tape-side adhesive layer is used. In the figure, 11 represents the base film of the release tape, 12 represents the adhesive layer of the release tape, 22 represents the release tape-side adhesive layer of the adhesive material, 21 represents the base film of the adhesive material, 23 represents the wafer-side adhesive layer of the adhesive material, and 3 represents the wafer.

[0109] The raw material of the base film of the bonding material is not particularly limited, but it is preferred to use a plastic film, for example, films, sheets, sheets with a mesh structure, sheets through perforations, etc. of acrylic acid, olefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, urethane, polyetheretherketone (PEEK), liquid crystal polymer (LCP), polyimide, polyester, fluororesin, etc. can be listed. From the viewpoint of operability, PET, PEN, or polyimide film is preferred.

[0110] Peel off tape

[0111] The release tape is used to release the adhesive material from the laminate A composed of the wafer and the adhesive material. The release tape used in the wafer manufacturing method of the present invention comprises at least a base film and an adhesive layer, and the adhesive layer contains a silicone adhesive component.

[0112] As the silicone adhesive component, polyorganosiloxane can be cited. The silicone adhesive includes a peroxide-curing adhesive obtained by adding silicone resin and organic peroxide to polyorganosiloxane, or an addition-curing adhesive obtained by mixing vinyl-containing polyorganosiloxane, silicone resin, and SiH-containing siloxane.

[0113] Silicone adhesives have the property of wetting and spreading independently of the adherend, so when the peeling tape is attached to the adhesive material of the laminate A composed of the wafer and the adhesive material, the peeling tape can be fully attached to the end of the adhesive material. By fully adhering to the end of the adhesive material, it can be easily peeled off from the end of the adhesive material, so compared with the prior art, it is easy to create the beginning of peeling, and the adhesive material can be stably peeled off from the laminate A composed of the wafer and the adhesive material.

[0114] Furthermore, from the viewpoint of adjusting the peel strength P1, the adhesive layer of the release tape may contain various adhesive components or additives in addition to the silicone-based adhesive component.

[0115] The raw material used for the base film of the release tape is not particularly limited, but it is preferred to use a plastic film, for example, films, sheets, sheets having a mesh structure, sheets with holes, etc. of acrylic, olefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, urethane, polyetheretherketone (PEEK), liquid crystal polymer (LCP), polyimide, polyester, fluororesin, etc. can be cited. From the viewpoint of adjusting the operability and the peeling strength P1, the base film of the release tape preferably includes at least one of polyimide, polyester, or fluororesin.

[0116] In the manufacture method of wafer of the present invention, by using the aforementioned peeling tape, the aforementioned adhesive material can be peeled off from the laminated body A consisting of the adhesive material and the wafer. The method for peeling off the adhesive material is not particularly limited, but for example, in the laminated body A consisting of the adhesive material and the wafer, the aforementioned peeling tape is evenly attached to the face A of the adhesive material, and one end of the aforementioned peeling tape is torn off relative to the face B in the direction of 10 ° to 180 °. The aforementioned peeling tape can be fully attached to the end of the adhesive material, so the adhesive material can be peeled off from the end. In addition, with the end of the adhesive material peeled off from the wafer as the beginning, it is also possible to peel off again by mechanical peeling, etc.

[0117] Wafer

[0118] In the wafer support system, the wafer is temporarily fixed to the support body using an adhesive material, and the back grinding and cutting of the wafer are processed as a stacked body B composed of the support body / adhesive material / wafer. After the wafer is processed, the support body is removed to obtain a stacked body A composed of the wafer and the adhesive material. In the manufacturing method of the wafer of the present invention, there is a step of peeling off the adhesive material using a peeling tape from the stacked body A composed of the wafer and the adhesive material. The wafer is not particularly limited, as long as it is a wafer generally used in a semiconductor manufacturing process, any one can be manufactured. Among them, due to reasons such as thinning or easy damage, it is necessary to pay attention to operability during this processing, and therefore, it is suitable for wafers that require temporary fixation. Here, the thinning or easy damage of the wafer can be preset, for example, in the case where the thickness is temporarily thinned in the middle of the processing, which causes obstacles to operability, and adhesive materials can be used for temporary fixation of such a wafer to the support body. Examples of temporary thinning include: starting with a thin wafer, thinning a somewhat thick wafer in the middle of a process, and further processing a thinned wafer. The thickness of a temporarily thinned wafer is usually 1 to 200 μm.

[0119] For example, after the processing of the functional layer is completed, the semiconductor wafer is temporarily fixed to the support body in a manner such that the functional layer becomes the support body side, the opposite side (back side) of the functional layer is thinly ground and cut, and ion implantation, annealing, and electrode formation are performed on the back side. In the case of separation from the support body, the semiconductor wafer in the step is equivalent to the wafer.

[0120] As described above, the wafers processed or manufactured by the manufacturing method of the present invention also include wafers whose states change during the manufacturing process.

[0121] As mentioned above, the wafers processed and manufactured using the wafer manufacturing method of the present invention are not particularly limited, but as a more specific example, semiconductor wafers may include silicon wafers, or compound semiconductor wafers such as SiC, AlSb, AlAs, AlN, AlP, BN, BP, BAs, GaSb, GaAs, GaN, GaP, InSb, InAs, InN, or InP, crystal wafers, sapphire, glass, molded wafers, etc.

[0122] Silicon wafers or compound semiconductor wafers may be doped.

[0123] An electrical / electronic functional layer may be formed on or in the wafer. Examples of suitable functional layers include electronic circuits, capacitors, transistors, resistors, electrodes, optical elements, MEMS, etc., but may also be micro devices other than these.

[0124] The surfaces of these functional layers are formed of one or more of the following raw materials, and may typically have structures belonging to electrodes. Examples of the raw materials for the functional layers include silicon, polysilicon, silicon dioxide, (oxy) silicon nitride, metals (e.g., copper, aluminum, gold, tungsten, tantalum), low-k dielectrics, polymer dielectrics, and various metal nitrides and metal silicides. The surface (functional layer surface) on which the functional layer side of the wafer is formed may also have structures such as solder bumps, metal columns, and bumps.

[0125] In addition, in order to form a functional layer or to protect the functional layer, the wafer surface may be covered with an oxide film or a nitride film. In addition, the wafer surface may be covered with a passivation film for wafer protection.

[0126] The wafer manufactured by the wafer manufacturing method of the present invention is further supplied to the subsequent steps to manufacture the final product. When the functional layer is formed on the wafer, the steps commonly used in the manufacture of electronic devices such as semiconductor devices, such as dicing, packaging, and sealing, can be performed to manufacture the final product.

[0127] In the measurement of the peel strength P2 of the present invention, as described above, a polyimide coated wafer is used as a wafer for measurement. The adhesive strength between the adhesive material / wafer will vary depending on the presence or absence of a functional layer or film on the surface of the wafer, but if the peel strength P2 of the polyimide coated wafer used as the wafer for measurement is within a predetermined range, then among various wafers generally used in the wafer manufacturing process, the peel strength ratio P1 / P2 will not be significantly affected, and the adhesive material can be appropriately peeled.

[0128] Laminated body A

[0129] According to the manufacturing method of the wafer of the present invention, the adhesive material can be peeled off from the stacked body A composed of the adhesive material and the wafer to obtain the wafer. The stacked body A composed of the adhesive material and the wafer is obtained by, for example, fixing the support to the surface A of the adhesive material and fixing the wafer to the surface B, obtaining the stacked body B composed of the support / adhesive material / wafer, and then removing the support. The stacked body B composed of the support / adhesive material / wafer has sufficient strength and rigidity to prevent bending or breakage, and at the same time, the wafer is supplied to various semiconductor manufacturing processes.

[0130] The method for forming the stacked body B composed of support body / adhesive material / wafer is to stack the support body, adhesive material, and wafer in sequence. The stacking order is not particularly limited, and these layers can be stacked at once or in sequence.

[0131] When the adhesive is supplied as a liquid curable adhesive, the liquid curable adhesive can be applied to either the wafer or the support, or both of them by spin coating, etc., to form an adhesive or an adhesive precursor, and then a laminate is further produced.

[0132] When the adhesive or the adhesive precursor is supplied as a solid film, the bonding strength to the support is usually set lower than that to the wafer side. Therefore, from the perspective of preventing peeling during handling, it is preferred to first stick the film to the wafer and then stack the support.

[0133] When the film is attached at normal pressure and the formation of the laminate is carried out while reducing the pressure, it is preferred to first attach the film to a support and then to affix it to the wafer from the viewpoint of improving the absorption of the irregularities of the wafer.

[0134] When the adhesive material or the adhesive material precursor contains a curable adhesive component, the curable adhesive component can be irradiated with light or heated during formation of the laminate to crosslink and cure the curable adhesive component to cure the adhesive material.

[0135] The chemical resistance of the curing adhesive component that is cross-linked and hardened by light irradiation or heating will be greatly improved, and even if the back of the wafer is treated with a chemical solution during the wafer processing step, the adhesive material can be suppressed from eluting into the chemical solution. In addition, the elastic coefficient of the curing adhesive component that is cross-linked and hardened will increase, so it is not easy to deteriorate the bonding even at high temperature, and it is easier to peel off.

[0136] Thus, in this embodiment, although the wafer is subjected to heat treatment, mechanical processing, and / or wet treatment in the wafer processing steps, sufficient bonding force is maintained during the wafer processing, and after the wafer processing steps are completed, the support body is removed from the stack B, and the wafer is peeled off from the stack A without damaging the wafer or generating residual adhesive, and can be peeled off from the adhesive material.

[0137] For example, when an adhesive component containing a polymer having an unsaturated double bond such as a vinyl group in a side chain and a photopolymerization initiator activated at a wavelength of 250 to 800 nm is used as a light-curing adhesive component that is crosslinked and cured by the above-mentioned light irradiation, it is preferred that such a light-curing adhesive component be irradiated with an illuminance of 5 mW or more, more preferably 10 mW or more, still more preferably 20 mW or more, and particularly preferably 50 mW or more. In addition, it is preferred that the irradiation be performed with a cumulative irradiance of 300 mJ or more, more preferably 500 mJ or more and 10,000 mJ or less, still more preferably 500 mJ or more and 7,500 mJ or less, and particularly preferably 1,000 mJ or more and 5,000 mJ or less.

[0138] In addition, for example, when an adhesive material or an adhesive material precursor is a thermosetting adhesive component that is cross-linked and hardened by the above-mentioned heating, and an adhesive material is used that contains: a polymer having an unsaturated double bond such as a vinyl group in a side chain, and a thermal polymerization initiator that is activated by heating at about 50 to 200°C, the above-mentioned thermosetting adhesive component can be cross-linked and hardened by heating at a temperature of about 50 to 200°C for 10 to 60 minutes.

[0139] As described above, when the adhesive material is formed by hardening the precursor of the adhesive material, it can be stacked with the support or wafer after hardening, and can be hardened after stacking, and can be stacked in a semi-hardened state and finally hardened.

[0140] The method for removing the support from the laminate B composed of the support / adhesive material / wafer is not particularly limited, but from the perspective of cost or convenience, it is preferably removed by mechanical peeling. The method for mechanical peeling is not particularly limited, and peeling can be appropriately performed using a commercially available device or the like.

[0141] Support

[0142] In the manufacturing method of the wafer of the present invention, before the step of peeling off the aforementioned adhesive material from the stacked body A consisting of the wafer and the adhesive material, the wafer and the support can be temporarily fixed using the adhesive material, and the processing steps such as back grinding and cutting of the wafer can be performed. As a support, it is preferred to have sufficient strength and rigidity, and to have excellent heat resistance and chemical resistance. By using such a support, even when the wafer is thinly ground and cut, the wafer can be stably operated without bending, etc., and the wafer can be supplied to a plurality of and / or multiple processes. For example, in order to manufacture various processes required for an electronic device having a structure of a semiconductor chip (chip) stacked with TSV connections, etc., a wafer formed with an electronic circuit can be supplied.

[0143] Preferred raw materials used in the support include silicon, sapphire, crystal, metal (e.g., aluminum, copper, steel), and various glasses and ceramics. The support may be composed of a single raw material, but may also be composed of multiple raw materials, and may include other raw materials deposited on the substrate. For example, a vapor-deposited layer of silicon nitride or the like may be provided on a silicon wafer. The surface may be treated by providing a silicone layer or the like.

[0144] The support may be made of plastic depending on the temperature of the process of supplying the laminate. For example, a sheet made of plastic such as polyimide, acrylic acid, polyolefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), nylon, urethane, etc. is preferably used as the support. Polyimide can be used because it has a certain degree of heat resistance.

[0145] In order to obtain uniform thickness of the wafer after grinding and cutting, it is desirable that the thickness of the support body is uniform. For example, in order to thin a silicon wafer to less than 50 μm and make its uniformity less than ±10%, the thickness variation of the support body should be suppressed to less than ±2 μm.

[0146] The thickness of the support is not particularly limited, but from the viewpoint of effectively preventing the wafer from bending, it is preferably 300 μm or more, and particularly preferably 500 μm or more. From the viewpoint of suppressing the total weight during operation or reducing the stress required for mechanical peeling, it is preferably 1500 μm or less, and particularly preferably 1000 μm or less.

[0147] In addition, the present invention is not limited to the method of manufacturing a wafer.

[0148] A peeling method is also provided, which is a method for peeling the adhesive material from a laminated body A consisting of a wafer and an adhesive material using a peeling tape.

[0149] The release tape used in the release method contains a silicone adhesive component in the adhesive layer in contact with the adhesive material.

[0150] The adhesive material used in the peeling method has P1 and P2 satisfying a peel strength ratio P1 / P2 of 6 or more and P2 of 0.5 N / 25 mm or more;

[0151] Among them, the above-mentioned adhesive material has a surface A connected to the above-mentioned release tape and a surface B connected to the wafer, P1 is the peel strength of surface A when the above-mentioned release tape is measured at 90° relative to the above-mentioned adhesive material, and P2 is the peel strength of surface B when the above-mentioned adhesive material is measured at 90° relative to the polyimide coated wafer.

[0152] The peeling method of the present invention is not limited to the wafer manufacturing step. For example, when a thin wafer is transported, if an adhesive is used to protect the wafer, the adhesive used for protection can be stably peeled off from the stacked body A composed of the wafer and the adhesive. In this aspect, the adhesive can be in the form of a protective tape having an adhesive layer.

[0153] The peel strengths between the release tape / adhesive and between the adhesive / wafer used in the peeling method of the present invention are measured under the conditions described above. From the viewpoint of contact with the adhesive at the surface A, the release tape contains a silicone adhesive component in the adhesive layer.

[0154] The adhesive material used in the peeling method of the present invention is not particularly limited as long as it satisfies the above conditions, but it is preferred that the layer having the surface A of the adhesive material contains a silicone-based adhesive component or a silicone release agent.

[0155] The silicone compound contained in the silicone release agent has excellent heat resistance, so even after being treated with heating at more than 200°C, it can prevent the adhesive from being burned, etc., and it can easily be peeled off by seeping out to the interface of the adherend during peeling. In addition, the silicone compound has a curable adhesive and a cross-linkable functional group that can be contained as an adhesive component. Due to light irradiation or heating, it reacts chemically with the aforementioned curable adhesive and is introduced into the aforementioned curable adhesive, so the silicone compound will not adhere to the adherend and cause contamination. In addition, by deploying the silicone compound, it can also play an effect of preventing residual glue on the wafer.

[0156] In particular, when the layer having the surface A of the adhesive material is an adhesive layer, the adhesive layer preferably contains a silicone release agent from the viewpoint of adjusting the adhesive strength with the release tape. The adhesive layer particularly preferably contains an acrylic adhesive component containing a silicone release agent. The silicone release agent makes it easy to adjust the adhesive strength while maintaining heat resistance.

[0157] The aforementioned adhesive material used in the stripping method of the present invention preferably has at least a wafer side adhesive layer, a base film, and a stripping tape side adhesive layer. For the adhesive component used in the wafer side adhesive layer and the stripping tape side adhesive layer, the aforementioned component can be used. In addition, the aforementioned base film can also be used for the base film.

[0158] According to the present invention, an adhesive material can be provided, which is used in the above-mentioned wafer manufacturing method or peeling method, and has a peel strength P2 of 0.5N / 25mm or more. Here, the measurement conditions of the peel strength P2 and the composition of the adhesive material are as described above.

[0159] The peel strength P2 of the adhesive material of the present invention is 0.5 N / 25 mm or more, and preferably 0.7 N / 25 mm or more.

[0160] The upper limit of the peel strength P2 is not particularly limited as long as the above-mentioned peel strength ratio P1 / P2 is satisfied, but is preferably 2.5 N / 25 mm or less, and more preferably 2 N / 25 mm or less.

[0161] By setting the peel strength P2 to be 0.5N / 25mm or more, the wafer can be prevented from peeling off from the support during the wafer thin grinding and cutting process. By setting the peel strength P2 to be 2N / 25mm or less, when peeling the adhesive from the wafer, unexpected peeling of the peeling tape and the adhesive and residual adhesive on the wafer can be prevented.

[0162] From the viewpoint of adjusting the peel strength P1 between the release tape / adhesive material, in the adhesive material of the present invention, the layer having the surface A of the aforementioned adhesive material in contact with the release tape may contain a silicone adhesive component or a silicone release agent. By having the layer having the surface A contain a silicone adhesive component or a silicone release agent, the release tape is bonded to the end of the adhesive material, and it is easy to create a start when peeling the adhesive material from the wafer, so the adhesive material can be more easily peeled from the laminate A composed of the wafer and the adhesive material. The silicone adhesive component and silicone release agent that can be used in the adhesive material of the present invention are as described above.

[0163] In addition, according to the present invention, there is provided a release tape used in the above-mentioned wafer manufacturing method or release method, wherein the release tape has at least a base film and an adhesive layer, and the adhesive layer contains a silicone-based adhesive.

[0164] The adhesive layer of the release tape of the present invention contains a silicone-based adhesive component.

[0165] As the aforementioned silicone adhesive component, polyorganosiloxane can be cited. Silicone adhesives include: peroxide-hardening adhesives formed by adding silicone resin and organic peroxide to polyorganosiloxane, or addition-hardening adhesives formed by mixing polyorganosiloxane containing vinyl, silicone resin, and SiH-containing siloxane. Since silicone adhesives have the property of wetting and spreading independently of the adherend, the silicone adhesive component is contained in the adhesive layer by the peeling tape, and it can be fully attached to the end of the adhesive material. Therefore, by fully adhering to the end of the adhesive material, it can be easily peeled off from the end of the adhesive material.

[0166] The raw material used for the base film of the release tape is not particularly limited, and the above-mentioned raw materials can be used. From the viewpoint of adjusting the workability and the peel strength P1, the base film of the release tape preferably contains at least one of polyimide, polyester, or fluororesin.

[0167] [Example]

[0168] The present invention will be described in detail below. In addition, the present invention is not limited to the following examples in any sense.

[0169] The physical properties and characteristics of Examples and Comparative Examples were evaluated according to the following methods.

[0170] (1) Evaluation of the removability of adhesive materials from wafers

[0171] (1-1) Preparation of Laminated Body A

[0172] A stacked body B is prepared by stacking the support body 7 / adhesive material 23 (for simplicity, a single-layer structure is shown in the figure) / wafer 3 in this order using a silicon wafer as a support body 7 and a polyimide-coated wafer as a wafer 3. The stacked body B is subjected to a heat treatment at 140° C. for 30 minutes and then to a heat treatment at 200° C. for 30 minutes. The stacked body B is then fixed at room temperature on a dicing tape 5 attached to a ring frame 6 with the polyimide-coated wafer side facing downward. The dicing tape 5 is fixed by a vacuum clamp ( Figure 3 In order to peel off the interface between the silicon wafer belonging to the support 7 and the adhesive material 23, the removal tool 8 is slid into the interface between the support 7 and the adhesive material 23, and an upward force of typically about 120N or less is applied to the end of the silicon wafer belonging to the support, thereby forming a peeling interface ( Figure 3 (b) of the Regulations).

[0173] Then, pressure is applied to the formed peeling interface ( Figure 3 (c) part), and expand the peeling interface to peel off the silicon wafer belonging to the support body 7, thereby producing a stacked body A composed of the wafer and the adhesive material.

[0174] (1–2) Evaluation

[0175] For the laminate A consisting of wafer 3 / adhesive material 23 (for simplicity, shown as a single-layer structure) fixed to the dicing tape 5 attached to the ring frame 6, a peeling tape consisting of a base film 11 of the peeling tape and an adhesive layer 12 of the peeling tape is attached to the entire surface of the adhesive material 23. The dicing tape 5 is fixed with a vacuum clamp, and the peeling tape consisting of 11 and 12 is pulled up at a peeling angle of 90° and a peeling speed of 5 mm / s to peel off the adhesive material 23. The peelability is evaluated according to the following criteria ( Figure 4 ).

[0176] ○: The adhesive material can be completely peeled off from the wafer without causing damage to the wafer.

[0177] ×: The adhesive material cannot be peeled off from the wafer.

[0178] (2) Determination of peel strength P1 (peel strength at surface A between peel tape / adhesive material)

[0179] (2-1) Preparation of P1 measurement samples

[0180] The adhesive material 1 or adhesive material 2 described later is cut into 3 cm × 5 cm, and is attached to the silicon wafer belonging to the support in a manner that the adhesive layer on the side of the peeling tape is opposite. The adhesive layer on the wafer side is attached with a polyethylene terephthalate film (separation membrane) treated with silicone release (laminate C). After heating laminate C at 140°C for 30 minutes, it is heated at 200°C for 30 minutes as a condition of pretreatment in the formation step of the preset laminate A. Thereafter, the P1 measurement sample is obtained by removing the separation membrane and the silicon wafer.

[0181] (2–2) Determination

[0182] The wafer-side adhesive layer of the P1 measurement sample prepared in the above (2-1) is attached to an acrylic plate (not shown) via a commercially available double-sided tape. The adhesive layer 12 of the release tape cut into 3 cm × 6 cm is attached to the release tape-side adhesive layer 22 of the P1 measurement sample, and the release tape is cut into 2.5 cm width per P1 measurement sample. Thereafter, a 2 kg roller is used to pressurize the sample back and forth. The peel strength P1 (part (a) of Figure 1) is measured at 22.5 ± 1 ° C and a relative humidity of 50 ± 10% using VPA-S (manufactured by Kyowa Interface Science Co., Ltd.) at a tensile speed of 300 mm / min and a peeling angle of 90°.

[0183] (3) Measurement of peel strength P2 (peel strength at surface B between adhesive material and wafer)

[0184] (3-1) Preparation of samples for P2 measurement

[0185] The adhesive material 1 or adhesive material 2 described later is cut into 3 cm × 5 cm, and attached to the polyimide coated wafer in a manner that the wafer side adhesive layer is opposite, and then pressed back and forth with a 2 kg roller 1. The adhesive layer on the release tape side is attached with a polyethylene terephthalate film (separation film) treated with silicone release (laminate D). After heating laminate D at 140 ° C for 30 minutes, it is heated at 200 ° C for 30 minutes as a pretreatment condition in the formation step of the preset laminate A. Thereafter, the separation film on the adhesive layer on the release tape side is removed to obtain a sample for P2 measurement.

[0186] (3–2) Determination

[0187] The P2 measurement sample prepared in the above (3-1) was cut into 2.5 cm × 5 cm, and the peel strength P2 was measured at 22.5±1°C and a relative humidity of 50±10% using VPA-S (manufactured by Kyowa Interface Science Co., Ltd.) at a tensile speed of 300 mm / min and a peel angle of 90 degrees (part (b) of Figure 1).

[0188] Details of materials and raw materials used in Examples and Comparative Examples are as follows.

[0189] Support and wafer

[0190] In the confirmation of the removability of the adhesive material, a silicon wafer and a polyimide-coated wafer were used as the support and the wafer.

[0191] Silicon wafer

[0192] A Si mirror wafer with an outer diameter of 150 mm and a thickness of 625 μm was used.

[0193] Polyimide coated wafer

[0194] A wafer having a polyimide film of 5 μm thick provided on a Si mirror wafer of 150 mm in outer diameter and 625 μm in thickness was used.

[0195] Wafer for measuring peel strength P2

[0196] The following wafers were used for the measurement of the peel strength P2.

[0197] Polyimide coated wafer

[0198] A wafer having a polyimide film of 5 μm thick provided on a Si mirror wafer of 150 mm in outer diameter and 625 μm in thickness was used.

[0199] Peel off tape

[0200] The following release tapes were used in Examples and Comparative Examples.

[0201] ·Release tape 1: No.360UL (manufactured by Nitto Denko Co., Ltd.)

[0202] ·Release tape 2: 5413 (manufactured by 3M JAPAN Co., Ltd.)

[0203] ·Release tape 3: 8992 (manufactured by 3M JAPAN Co., Ltd.)

[0204] Release tape 4: MHM-SI25 (manufactured by Nichiei Shinka Co., Ltd.) was backed with a 50 μm PET film.

[0205] · Peeling tape 5: ASF116T FR (manufactured by Chung Hsing Chemical Industry Co., Ltd.)

[0206] ·Peeling tape 6: No.31B (manufactured by Nitto Denko Co., Ltd.)

[0207] Release tape 7: VHB BR-12 (manufactured by 3M JAPAN Co., Ltd.) was backed with a 50 μm PET film.

[0208] ·Release tape 8: Cellotape (registered trademark) (manufactured by NICHIBAN Co., Ltd.)

[0209] Resin for forming adhesive layer

[0210] The resin used to form the adhesive layer of the adhesive material is adjusted as follows.

[0211] ·(Meth)acrylic resin solution N

[0212] 49 parts by mass of ethyl acrylate, 20 parts by mass of 2-ethylhexyl acrylate, 21 parts by mass of methyl acrylate, 10 parts by mass of glycidyl methacrylate, and 0.5 parts by mass of a benzoyl peroxide-based polymerization initiator as a polymerization initiator were reacted at 80° C. for 10 hours in a solvent consisting of 65 parts by mass of toluene and 50 parts by mass of ethyl acetate. After the reaction was completed, the obtained solution was cooled, and 25 parts by mass of xylene, 5 parts by mass of acrylic acid, and 0.5 parts by mass of tetradecyldimethylbenzyl ammonium chloride were added to the cooled solution, and the mixture was reacted at 85° C. for 32 hours while blowing air, thereby obtaining a (meth)acrylic resin solution N.

[0213] Substrate film

[0214] The following films were used as the base film used for the bonding material.

[0215] ·PEN film

[0216] A polyethylene naphthalate film (corona-treated on both sides, thickness: 50 μm, manufactured by Toyobo Film Solutions Co., Ltd., TEONEX Q83) was used.

[0217] PET film

[0218] A biaxially stretched polyethylene terephthalate film (corona-treated on both sides, thickness 38 μm, manufactured by TORAY CO., LTD., LUMIRROR S10) was used.

[0219] Polyimide film

[0220] A polyimide film (double-sided plasma treatment, thickness 38 μm, manufactured by TORAY DUPONT CO., LTD., trade name: KAPTON (registered trademark) 150EN-A) was used.

[0221] Adhesive materials 1

[0222] 2.84 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 50 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), 2.0 parts by mass of silicone diacrylate (manufactured by DAICEL ALLNEX Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of PERKADOX 12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to 270 parts by mass of the (meth)acrylic resin solution N to obtain a coating liquid 1-1 for an adhesive layer on the support side (release tape side). The coating liquid 1-1 was applied to a base film (PEN film) and dried at 100° C. for 10 minutes to form an adhesive layer 1-1 having a thickness of 25 μm as an adhesive layer on the support side (release tape side). Then, a polyethylene terephthalate film (separator film) subjected to silicone release treatment was laminated to obtain a laminate consisting of the adhesive layer 1-1 / base film with a separator film.

[0223] To 270 parts by mass of (meth)acrylic resin solution N, 0.1 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), 0.5 parts by mass of silicone diacrylate (manufactured by DAICEL ALLNEX Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of PERKADOX 12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to obtain a coating liquid 1-2 for an adhesive layer on the wafer side. The coating liquid 1-2 was applied to a polyethylene terephthalate film (release film) subjected to a silicone release treatment and dried at 100° C. for 10 minutes to form an adhesive layer 1-2 having a thickness of 40 μm as an adhesive layer on the wafer side. Then, the adhesive layer 1-2 is bonded to the substrate side of the laminate composed of the adhesive layer 1-1 / substrate film to obtain a three-layer laminate composed of the adhesive layer 1-1 / substrate film / adhesive layer 1-2 with a separator.

[0224] To 270 parts by mass of (meth)acrylic resin solution N, 5.68 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), 0.5 parts by mass of silicone diacrylate (manufactured by DAICEL ALLNEX Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of PERKADOX 12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to obtain a coating liquid 1-3 for an adhesive layer on the wafer side. The coating liquid 1-3 was applied to a polyethylene terephthalate film (release film) subjected to a silicone release treatment and dried at 100° C. for 10 minutes to form an adhesive layer 1-3 having a thickness of 10 μm as an adhesive layer on the wafer side. Then, by bonding the adhesive layer 1-3 to the adhesive layer 1-2 side of the above-mentioned laminated body composed of three layers of the adhesive layer 1-1 / base film / adhesive layer 1-2 with a separation membrane, a precursor of the adhesive material 1 before heat treatment, which is composed of four layers of the adhesive layer 1-1 / base film / adhesive layer 1-2 / adhesive layer 1-3 with a separation membrane, is prepared.

[0225] Bonding materials 2

[0226] 2.84 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 50 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), 2.0 parts by mass of polyether-modified polydimethylsiloxane containing an acrylic group (manufactured by BYKCHEIME JAPAN Co., Ltd., trade name: BYK-UV3500), and 2 parts by mass of PERKADOX 12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to 270 parts by mass of the (meth)acrylic resin solution N to obtain a coating liquid 2-1 for an adhesive layer on the support side (release tape side). The coating liquid 2-1 was applied to a base film (PEN film) and dried at 100° C. for 10 minutes to form an adhesive layer 2-1 having a thickness of 25 μm as an adhesive layer on the support side (release tape side). Then, a polyethylene terephthalate film (separator film) subjected to silicone release treatment was laminated to obtain a laminate consisting of the adhesive layer 2-1 / base film with a separator film.

[0227] To 270 parts by mass of (meth)acrylic resin solution N, 0.1 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), and 2 parts by mass of PERKADOX12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to obtain a coating liquid 2-2 for an adhesive layer on the wafer side. The coating liquid 2-2 was applied to a polyethylene terephthalate film (separation film) subjected to a silicone release treatment and dried at 100° C. for 10 minutes to form an adhesive layer 2-2 having a thickness of 40 μm as an adhesive layer on the wafer side. Then, the adhesive layer 2-2 is bonded to the substrate side of the laminate composed of the adhesive layer 2-1 / substrate film, thereby obtaining a three-layer laminate composed of the adhesive layer 2-1 / substrate film / adhesive layer 2-2 with a release membrane.

[0228] 5.68 parts by mass of HDI isocyanurate (manufactured by TOSOH Co., Ltd., trade name: CORONATE HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Toagosei Co., Ltd., trade name: ARONIX M-402), and 2 parts by mass of PERKADOX12XL25 manufactured by Kayaku NOURYON Co., Ltd. were added to 270 parts by mass of (meth)acrylic resin solution N to obtain a coating liquid 2-3 for an adhesive layer on the wafer side. The coating liquid 2-3 was applied to a polyethylene terephthalate film (separation film) treated with silicone release, and dried at 100° C. for 10 minutes to form an adhesive layer 2-3 with a thickness of 10 μm as an adhesive layer on the wafer side. Then, by bonding the adhesive layer 2-3 to the adhesive layer 2-2 side of the above-mentioned laminated body with a separation membrane composed of three layers of adhesive layer 2-1 / base film / adhesive layer 2-2, a precursor of the adhesive material 2 before heat treatment, which is composed of four layers of adhesive layer 2-1 / base film / adhesive layer 2-2 / adhesive layer 2-3 with a separation membrane, is prepared.

[0229] (Example 1)

[0230] Using the adhesive material 1 and the release tape 1, the peel strengths P1 and P2 were measured according to the above-mentioned peel strength measurement, and P1 / P2 was calculated. The result was P1 / P2=6.6.

[0231] Furthermore, based on the confirmation of the removability of the adhesive material from the above-mentioned wafer, the removability of the adhesive material 1 from the wafer was analyzed. As a result, the adhesive material 1 could be completely peeled off from the wafer without causing damage to the wafer.

[0232] (Example 2)

[0233] The peeling strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 2 was used. P1 / P2=6.8, indicating that the adhesive material 1 could be completely peeled off from the wafer without causing damage to the wafer.

[0234] (Example 3)

[0235] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 3 was used. P1 / P2=7.8, indicating that the adhesive material 1 could be completely peeled off from the wafer without causing damage to the wafer.

[0236] (Example 4)

[0237] The peeling strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 4 was used. P1 / P2=11.9, indicating that the adhesive material 1 could be completely peeled off from the wafer without causing damage to the wafer.

[0238] (Example 5)

[0239] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the adhesive material 2 was used. P1 / P2=9.6, indicating that the adhesive material 2 could be completely peeled off from the wafer without causing damage to the wafer.

[0240] (Example 6)

[0241] The peel strengths P1 and P2 were measured in the same manner as in Example 2 except that the adhesive material 2 was used. P1 / P2=9.3, indicating that the adhesive material 2 could be completely peeled off from the wafer without causing damage to the wafer.

[0242] (Example 7)

[0243] The peel strengths P1 and P2 were measured in the same manner as in Example 3 except that the adhesive material 2 was used. P1 / P2=10.7, indicating that the adhesive material 2 could be completely peeled off from the wafer without causing damage to the wafer.

[0244] (Example 8)

[0245] The peel strengths P1 and P2 were measured in the same manner as in Example 4 except that the adhesive material 2 was used. P1 / P2=16.2, indicating that the adhesive material 2 could be completely peeled off from the wafer without causing damage to the wafer.

[0246] (Comparative Example 1)

[0247] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the adhesive material 5 was used. P1 / P2=4.2, and the adhesive material 1 could not be peeled from the wafer.

[0248] (Comparative Example 2)

[0249] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 6 was used. P1 / P2=5.0, and the adhesive material 1 could not be peeled from the wafer.

[0250] (Comparative Example 3)

[0251] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 7 was used. P1 / P2=10.0, and the adhesive material 1 could not be peeled off from the wafer.

[0252] (Comparative Example 4)

[0253] The peel strengths P1 and P2 were measured in the same manner as in Example 1 except that the peeling tape 8 was used. P1 / P2=6.2, and the adhesive material 1 could not be peeled off from the wafer.

[0254] (Comparative Example 5)

[0255] Except for using the adhesive material 2, the peel strengths P1 and P2 were measured in the same manner as in Comparative Example 1. P1 / P2=5.4, and the adhesive material 2 could not be peeled from the wafer.

[0256] (Comparative Example 6)

[0257] Except for using the adhesive material 2, the peel strengths P1 and P2 were measured in the same manner as in Comparative Example 2. P1 / P2=4.3, and the adhesive material 2 could not be peeled from the wafer.

[0258] (Comparative Example 7)

[0259] Except for using the adhesive material 2, the peel strengths P1 and P2 were measured in the same manner as in Comparative Example 3. P1 / P2=12.3, and the adhesive material 2 could not be peeled from the wafer.

[0260] (Comparative Example 8)

[0261] Except for using the adhesive material 2, the peel strengths P1 and P2 were measured in the same manner as in Comparative Example 4. P1 / P2=7.1, and the adhesive material 2 could not be peeled from the wafer.

[0262] Tables 1 and 2 show the combinations of the release tape and the adhesive material used in each of the Examples and Comparative Examples, the results of the peel strength measurement, and the results of the evaluation of the removability of the adhesive material from the wafer.

[0263] [Table 1]

[0264] Table 1

[0265]

[0266] [Table 2]

[0267] Table 2

[0268]

[0269] [Industrial Application Possibility]

[0270] According to the method for manufacturing a wafer using a release tape and an adhesive material, and the release tape and the adhesive used in the method, it is possible to implement a plurality and / or a variety of steps on the wafer with high productivity and yield without causing damage to electronic components such as functional layers formed on the wafer, thereby making a significant contribution to improving the productivity of electronic devices and having high applicability in various fields of industries such as the electronic components industry headed by the semiconductor process industry, the power electronics industry using electronic components, the transportation machinery industry, the information and communication industry, and the precision machinery industry.

[0271] Description of Reference Numerals

[0272] 11: Remove the backing film of the tape

[0273] 12: Peel off the adhesive layer of the tape

[0274] 21: Base film for bonding materials

[0275] 22: Adhesive layer on the peeling tape side of the bonding material

[0276] 23: Wafer side adhesive layer of adhesive material or adhesive material with single layer structure

[0277] 3: Wafer

[0278] 5: Cutting tape

[0279] 6: Ring frame

[0280] 7: Support body

[0281] 8: Disassembly tool.

Claims

1. A method for manufacturing a wafer, comprising: A step of peeling the adhesive material from a laminate A consisting of a wafer and an adhesive material using a peeling tape; The release tape used in the step contains a silicone adhesive component in the adhesive layer in contact with the adhesive material. The adhesive material used in the step has a peel strength ratio P 1 / P 2 6 or above, and P 2 P of 0.5N / 25mm or more 1 and P 2 ; in, The adhesive material has a surface A in contact with the release tape and a surface B in contact with the wafer. 1 is the peel strength of the surface A when the peeling tape is held at 90° relative to the adhesive material, and P 2 It is the peel strength of the surface B when the adhesive is measured while being held at 90° with respect to the polyimide-coated wafer.

2. The method for manufacturing a wafer according to claim 1, in, The layer having the surface A of the adhesive material contains a silicone-based adhesive component or a silicone release agent.

3. The method for manufacturing a wafer according to claim 1 or 2, in, The adhesive material at least includes a wafer-side adhesive layer, a base film, and a release tape-side adhesive layer.

4. A peeling method, which is a method of peeling the adhesive material from a laminated body A consisting of a wafer and an adhesive material using a peeling tape, The release tape used in the release method contains a silicone adhesive component in the adhesive layer in contact with the adhesive material. The adhesive material used in the peeling method has a peel strength ratio P 1 / P 2 6 or above, and P 2 P of 0.5N / 25mm or more 1 and P 2 ; in, The adhesive material has a surface A in contact with the release tape and a surface B in contact with the wafer. 1 is the peel strength of the surface A when the peeling tape is held at 90° relative to the adhesive material, and P 2 It is the peel strength of the surface B when the adhesive is measured while being held at 90° with respect to the polyimide-coated wafer.

5. The stripping method according to claim 4, in, The layer having the surface A of the adhesive material contains a silicone-based adhesive component or a silicone release agent.

6. The peeling method according to claim 4 or 5, in, The adhesive material at least includes a wafer-side adhesive layer, a base film, and a release tape-side adhesive layer.

7. An adhesive material, which is an adhesive material used in the wafer manufacturing method or the wafer peeling method according to any one of claims 1 to 6, and P 2 It is 0.5N / 25mm or more. 8 . A release tape used in the wafer manufacturing method or release method according to claim 1 , wherein the release tape comprises at least a base film and an adhesive layer, wherein the adhesive layer contains a silicone adhesive.

9. The release tape according to claim 8, in, The base film of the release tape contains at least any one of polyimide, polyester, or fluororesin.