Lithium ion sieve subjected to surface modification by using phenylphosphinic acid and preparation method of lithium ion sieve
By using phenylphosphinic acid surface modification on lithium ion sieve, the problems of slow adsorption rate and low adsorption capacity of lithium ion sieve are solved, and the adsorption rate and cycle stability are improved. It is suitable for industrial applications, especially in complex salt lake brines In the environment.
Patent Information
- Application Number
- CN202411031246.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium ion sieves have slow adsorption rate, low actual adsorption capacity, and insufficient cycle stability, which limits their large-scale application in industrial production.
The preparation method of phenylphosphinic acid surface modified lithium ion sieve is adopted. By preparing lithium titanium oxide precursor and phenylphosphinic acid are mixed in a buffer solution and acid treatment is carried out to optimize the lithium source, titanium source and flux agent. The ratio of the heat treatment temperature and time are adjusted to improve the adsorption performance and cycling stability of the material.
The adsorption rate and adsorption capacity of lithium ion sieve are significantly improved. The material maintains a low titanium loss rate after multiple cycles. It is suitable for industrial applications and shows excellent performance in complex salt lake brine environments.
Smart Images

Figure CN118949910A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium ion sieves, and in particular to a lithium ion sieve surface-modified with phenylphosphinic acid and a preparation method thereof. Background Art
[0002] With the transformation of the global energy structure and the rapid development of the new energy vehicle industry, the demand for lithium resources has risen sharply. As a lightweight, high-energy-density element, lithium is known as the "industrial MSG" and plays a vital role in various industrial fields. Lithium resources are widely distributed, but are mainly concentrated in salt lake brine and land ores. Among them, the lithium resources in salt lake brine account for as much as 80%, far exceeding the total amount of lithium resources in land ores.
[0003] In the development and utilization of lithium resources, lithium extraction technology is a key link. At present, adsorption has become the most commonly used method for lithium extraction due to its simple operation and low cost. In particular, lithium ion sieves as adsorbents have attracted much attention due to their high selectivity and high adsorption capacity. Lithium ion sieves are mainly divided into two categories: manganese and titanium. The preparation principle is based on introducing lithium ions into manganese oxide or titanium oxide compounds to generate lithium manganese or lithium titanium composite oxides, namely lithium ion sieve precursors.
[0004] By acid washing to remove lithium ions from the precursor, a lithium ion sieve rich in regular lithium vacancies can be obtained. This material exhibits good lithium ion selectivity and can effectively adsorb lithium ions from lithium-containing solutions. The theoretical adsorption capacity of the lithium ion sieve is closely related to the lithium-manganese ratio or lithium-titanium ratio in its precursor. Studies have shown that the metatitanate lithium ion sieve H 2 TiO 3 It has the highest theoretical adsorption capacity, but in practical applications, its adsorption capacity is often lower than the theoretical value, and the adsorption rate is slow, and it takes a long time to reach equilibrium.
[0005] Although lithium ion sieves have shown great potential in lithium extraction, their practical application still faces some challenges. For example, problems with adsorption rate and equilibrium time limit their large-scale application in industrial production. In addition, the regeneration ability and cycle stability of lithium ion sieves are also key factors affecting their economy and sustainability. Therefore, developing new and efficient lithium ion sieve materials and improving their adsorption performance and cycle stability are of great significance to meet the growing demand for lithium resources.
[0006] The present invention aims to solve at least one of the deficiencies in the prior art and provide a lithium ion sieve surface modified with phenylphosphinic acid and a preparation method thereof, so as to improve the adsorption rate and equilibrium time and enhance the cyclic stability of the material. Summary of the invention
[0007] The object of the present invention is to provide a lithium ion sieve surface modified with phenylphosphinic acid and a preparation method thereof, so as to solve the technical problems of slow adsorption rate and low actual adsorption capacity of the lithium ion sieve in the prior art.
[0008] To achieve the above object, the present invention adopts the following technical solution:
[0009] The present invention provides a method for preparing a lithium ion sieve surface-modified by phenylphosphinic acid, comprising the following steps: S001, preparing a lithium titanium oxide precursor; S002, mixing the precursor with phenylphosphinic acid in a buffer solution; S003, subjecting the mixed material to acid treatment.
[0010] Furthermore, the process of preparing the lithium titanium oxide precursor in step S001 includes: mixing a mixture of a lithium source and a titanium source with a flux, adding a solvent for grinding, and performing heat treatment after drying.
[0011] Specifically, the lithium source is Li 2 CO 3 , titanium source is TiO 2 , the flux is LiCl.
[0012] More specifically, the molar ratio of the lithium source to the titanium source is 2:1.
[0013] Furthermore, the solvent is anhydrous ethanol.
[0014] Specifically, the heat treatment includes calcining at 70-90° C. for 0.6-1.5 hours and then heating to 600-700° C. for calcining for 2-6 hours.
[0015] Furthermore, the buffer solution in step S002 is a tris(hydroxymethyl)aminomethane buffer solution with a pH value of 7.5-9.5.
[0016] Specifically, the amount of phenylphosphinic acid added in step S002 is 0-50% of the mass of the precursor.
[0017] More specifically, the acid treatment in step S003 uses an acid solution of 0.1-0.5 mol·L-1 at 20-30° C. for 12-36 hours.
[0018] The present invention also provides a surface-modified lithium ion sieve, which is prepared by the above method.
[0019] The present invention introduces phenylphosphinic acid into the surface of the lithium ion sieve precursor for modification, effectively breaking the water layer on the surface of the adsorbent, reducing powder aggregation, and thus improving the adsorption capacity; the surface water layer is broken, reducing the interface mass transfer resistance of lithium ions, thereby promoting the ion exchange rate and significantly improving the adsorption rate. Compared with the unmodified lithium ion sieve, the modified lithium ion sieve of the present invention can reach the maximum adsorption capacity in a shorter time.
[0020] The present invention further improves the performance of the lithium ion sieve by optimizing the ratio of lithium source, titanium source and flux, and regulating the heat treatment temperature and time. The pH value is controlled by tris(hydroxymethyl)aminomethane buffer solution to ensure the stability of the modification process. The modification effect can be accurately controlled by adjusting the addition amount of phenylphosphinic acid and the acid treatment conditions. The experimental results show that within the addition amount range of phenylphosphinic acid described in the present invention, the adsorption efficiency of the modified lithium ion sieve is significantly improved, and the titanium dissolution rate is still kept low after multiple cycles of use, which provides the possibility for the long-term use of the lithium ion sieve in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a TG comparison curve diagram of the first embodiment of the present invention and the comparative example;
[0022] Figure 2 This is a SEM image of the precursor particles prepared in the first embodiment of the present invention;
[0023] Figure 3 This is the SEM image of the precursor particles prepared in the comparative example;
[0024] Figure 4 It is a comparison curve diagram of the XRD spectra of the first embodiment of the present invention and the comparative example;
[0025] Figure 5 It is a comparison curve diagram of FTIR spectra of the first embodiment of the present invention and the comparative example;
[0026] Figure 6 Schematic diagram of the equilibrium adsorption capacity of HTO and HTO-nBPA for lithium ions in LiOH solution and simulated salt lake brine;
[0027] Figure 7 Schematic diagram of the adsorption isotherms of HTO and HTO-BPA;
[0028] Figure 8 Schematic diagram of the change of adsorption capacity of HTO and HTO-BPA in LiOH over time;
[0029] Fig. 9 Schematic diagram of the change of adsorption capacity of HTO and HTO-BPA in simulated salt lake brine over time;
[0030] Fig.10 Schematic diagram of the effect of eluent acid concentration on the lithium ion adsorption capacity of HTO and HTO-BPA. DETAILED DESCRIPTION
[0031] A lithium ion sieve surface modified with phenylphosphinic acid and a preparation method thereof of the present invention will be described in more detail below, wherein preferred embodiments of the present invention are shown, and it should be understood that those skilled in the art can modify the present invention described herein while still achieving the beneficial effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art and not as a limitation of the present invention.
[0032] In the description of this specification, "one embodiment" or "some embodiments" etc. means that one or more embodiments of this specification include a specific feature, structure or characteristic described in conjunction with the embodiment. Therefore, the phrases "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. appearing in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways.
[0033] The present invention is described in more detail by way of example in the following paragraphs with reference to the accompanying drawings. Advantages and features of the present invention will become more apparent from the following description.
[0034] Example 1
[0035] This embodiment proposes a method for preparing a lithium ion sieve surface modified with phenylphosphinic acid, and the specific steps are as follows:
[0036] S001. preparing a lithium titanium oxide precursor;
[0037] S002, mixing the precursor with phenylphosphinic acid in a buffer solution;
[0038] S003. Treat the mixed material with acid.
[0039] Specifically, in S001, a lithium titanium oxide precursor is prepared: Li 2 CO 3 (Lithium carbonate) and TiO 2 (Anatase) as lithium source and titanium source, a stoichiometric mixture is prepared according to the molar ratio of Li:Ti = 2:1. LiCl is used as a flux and mixed with the above mixture. The preferred solute concentration (Li 2 CO 3The molar ratio of LiCl to LiCl was 50 mol%. 4 mL of anhydrous ethanol was added to the mixture and ground for 4 hours until no obvious granularity was observed. The obtained powder was dried at 60 ° C for 12 hours. It was then calcined at 80 ° C for 1 hour and then heated to 650 ° C for 4 hours. After cooling to room temperature, it was washed with deionized water and dried to obtain Li 2 TiO 3 Lithium ion sieve precursor, denoted as LTO.
[0040] In this step, using LiCl as a flux is an innovative point of the present invention. The introduction of the flux can reduce the melting point of the reaction system, promote the diffusion of reactants and the growth of crystals, thereby helping to improve the crystallinity and uniformity of the product. Selecting LiCl as a flux can also avoid the introduction of other metal ions and maintain the purity of the system.
[0041] In this embodiment, phenylphosphinic acid (BPA) is used for modification in S002: prepare a tris (hydroxymethyl)aminomethane (Tris) buffer solution and adjust the pH value to 8.5. Weigh 5g of LTO precursor and prepare Tris buffer solutions containing 0, 0.5g, 1g, 1.5g, 2g, and 2.5g of BPA, respectively. Add the LTO precursor to these solutions with different BPA contents, respectively. Stir slowly at room temperature for 4 hours, filter and dry at 60°C for 24 hours to obtain the modified precursor material LTO-BPA.
[0042] In this step, the modification with different contents of BPA is to study the effect of BPA dosage on material properties. By systematically adjusting the amount of BPA added, we can find the best modification conditions to obtain the lithium ion sieve material with the best performance.
[0043] Furthermore, acid treatment was used in S003: the modified precursor was added to a 0.25 mol / L hydrochloric acid solution and shaken at 150 rpm for 24 hours at 25°C to fully exchange ions and fully remove lithium ions from the precursor. The product was filtered, washed with deionized water until neutral, and dried at 60°C to obtain a modified lithium ion sieve, which was recorded as HTO-BPA.
[0044] Acid treatment is a key step in the preparation of lithium ion sieves. Through acid treatment, lithium ions in the precursor can be removed to form a structure with regular lithium vacancies, which are the key to the selective adsorption of lithium ions by lithium ion sieves. The selection of a hydrochloric acid concentration of 0.25 mol / L is the result of optimization, which can ensure sufficient lithium removal while minimizing damage to the material structure.
[0045] According to the above steps, we prepared a series of lithium ion sieve samples with different BPA modification amounts, which were recorded as HTO (unmodified), HTO-0.1BPA, HTO-0.5BPA, HTO-1BPA, HTO-1.5BPA, HTO-2BPA and HTO-2.5BPA.
[0046] In order to clearly reflect the progress of this embodiment over the prior art, the preparation steps of Comparative Example 1 are proposed for experimental comparison with this embodiment:
[0047] Preparation of Li 2 CO 3 and TiO 2 The stoichiometric mixture (Li:Ti=2:1) was ground for 4 hours until there was no obvious granularity. The obtained powder was dried at 60℃ for 12 hours. After calcination at 80℃ for 1 hour, the temperature was raised to 650℃ for calcination for 4 hours. After cooling to room temperature, the Li2TiO3 (lithium dititanate) ion sieve precursor was obtained by washing with water and drying.
[0048] 1. Thermogravimetric analysis:
[0049] Figure 1 This is a thermogravimetric analysis (TG) comparison diagram of this embodiment and comparative example 1. The results show that the modified sample has additional mass loss at a lower temperature, which is related to the decomposition of BPA, further confirming the successful introduction of BPA.
[0050] Specifically, the HTO sample has a mass loss of about 2% in the range of 100-200°C, which mainly corresponds to the removal of adsorbed water. In the range of 200-800°C, the mass remains basically stable, and the total mass loss does not exceed 5%.
[0051] HTO-BPA sample: There is also a mass loss of about 2% in the range of 100-200°C, corresponding to the removal of adsorbed water. An additional mass loss of about 3-4% occurs in the range of 200-400°C, which can be attributed to the thermal decomposition of BPA. In the range of 400-800°C, the mass is basically stable.
[0052] This result not only confirms the successful introduction of BPA, but also provides quantitative information about the content of BPA in the material. At the same time, it also shows that the BPA-modified material may show a certain degree of performance change in temperature applications below 400°C, which provides an important reference for temperature control in practical applications.
[0053] 2. Scanning electron microscope (SEM) analysis:
[0054] Figure 2 and Figure 3The SEM images of the precursor particles prepared in Example 1 and Comparative Example 1 are shown respectively. It can be observed that the particles of the sample modified with BPA have better dispersibility and smoother surface, which is beneficial to improving the specific surface area and adsorption performance of the material.
[0055] Further, Figure 2 (HTO-BPA): The particles are in a relatively regular polyhedral shape with clear edges and a smooth surface. The particles are well dispersed and rarely agglomerated. The particle size distribution is relatively uniform, with most of them in the range of 0.5-2μm.
[0056] Figure 3 (HTO): The particle shape is irregular, the edges are rough, and there are some small protrusions and depressions on the surface. There is a certain degree of agglomeration between the particles, forming some larger aggregates. The particle size distribution is wide, ranging from submicron to several microns.
[0057] This difference in microstructure can explain the excellent adsorption performance of the HTO-BPA sample. After BPA modification, the particle surface becomes smoother and the surface irregularities are reduced, which may help reduce the adsorption of water molecules on the surface, thereby reducing the barrier of the water layer to the adsorption of lithium ions. At the same time, good dispersion increases the effective specific surface area and provides more lithium ion adsorption sites.
[0058] 3. X-ray diffraction (XRD) analysis:
[0059] Figure 4 The XRD spectra of Example 1 and Comparative Example 1 are compared. The results show that the BPA-modified sample still retains Li 2 TiO 3 The crystal structure of the material is not changed during the modification process. Figure 4 It can be observed that the diffraction peaks of the HTO-BPA sample are basically consistent with those of the LTO sample, and are consistent with the standard Li 2 TiO 3 This shows that the introduction of BPA did not lead to significant changes in the crystal structure of the material, ensuring the basic skeleton structure and lithium ion exchange capacity of the material. However, we noticed that the diffraction peak intensity of the HTO-BPA sample was slightly reduced, which was due to the modification of the material surface by BPA, resulting in a slight decrease in crystallinity. This slight structural change may be beneficial to improving the specific surface area and adsorption performance of the material. The reason for citing HTO-2.5BPA in this figure for comparison with the comparative example is that the HTO-2.5BPA has the highest degree of modification. Generally speaking, the higher the degree of modification, the greater the impact on the crystallinity. This comparative experiment selects the modified material with this value for comparison, which further illustrates that the crystallinity of the modified materials with other BPA contents in Example 1 is basically unaffected.
[0060] 4. Fourier transform infrared spectroscopy (FTIR) analysis:
[0061] Figure 5 The FTIR spectra of Example 1 and Comparative Example 1 are compared. The characteristic peaks of BPA can be observed in the spectrum of the modified sample, confirming that BPA was successfully introduced into the material surface. Specifically, in the spectrum of the HTO-BPA sample, we can observe the following characteristic peaks:
[0062] 3300-3500cm -1 The broad peaks in the range correspond to the stretching vibrations of P-OH and Ti-OH;
[0063] 1600cm -1 The peaks near ,correspond to the C=C stretching vibration of the benzene ring;
[0064] 1430cm -1 The near peak corresponds to the stretching vibration of PC;
[0065] 1000-1100cm -1 The strong peaks in the range correspond to P=O and PO stretching vibrations.
[0066] The appearance of these characteristic peaks clearly indicates that BPA has been successfully bound to the surface of the lithium ion sieve. It is worth noting that the introduction of BPA did not significantly affect the basic skeleton structure of the material, which is reflected in the peaks from 400-700 cm -1 The retention of the Ti-O framework vibration peaks in the range can be confirmed.
[0067] 5. Adsorption performance test:
[0068] Figure 6 The equilibrium adsorption capacity of HTO and HTO-nBPA for lithium ions in LiOH solution and simulated salt lake brine was demonstrated. The results showed that HTO-0.5BPA exhibited the best adsorption performance, so the subsequent experiments focused on the adsorption performance of HTO-0.5BPA (HTO-BPA for short).
[0069] In this experiment, in LiOH solution, the equilibrium adsorption capacity of HTO-0.5BPA reached 54.58 mg / g, which was about 15.5% higher than that of unmodified HTO (47.23 mg / g).
[0070] In simulated salt lake brine, the adsorption capacity of HTO-0.5BPA was 39.76 mg / g, while that of HTO was 34.12 mg / g, an increase of about 16.5%.
[0071] The effect of BPA dosage on adsorption performance showed a trend of increasing first and then decreasing, and the best effect was achieved when 0.5g BPA was used. This may be because too much BPA would occupy some adsorption sites and reduce the adsorption capacity.
[0072] 6. Adsorption isotherms of HTO and HTO-BPA:
[0073] Figure 7 The adsorption isotherms of HTO and HTO-BPA are shown. It can be seen from the figure that:
[0074] The adsorption isotherms of the two materials were consistent with the Langmuir model, indicating that the adsorption process was monolayer adsorption.
[0075] The isotherm of HTO-BPA is located above that of HTO in the entire concentration range, indicating that it has a higher adsorption capacity.
[0076] In the low concentration region (<50 mg / L), the adsorption amount of HTO-BPA increased faster, indicating that it is more effective in adsorbing low concentration lithium ions.
[0077] 7. Adsorption kinetics of HTO and HTO-BPA in LiOH:
[0078] Figure 8 The adsorption kinetic curves of HTO and HTO-BPA in LiOH (the adsorption capacity of HTO and HTO-BPA in LiOH changes with time) are shown. It can be observed that HTO-BPA can reach the maximum adsorption capacity within 1 hour, while HTO needs 5 hours to approach the maximum adsorption capacity. This proves that BPA modification significantly improves the adsorption rate of the material. The specific analysis is as follows:
[0079] The adsorption of HTO-BPA increased sharply in the first 30 minutes and basically reached equilibrium after 1 hour, with an adsorption capacity of 54.58 mg / g.
[0080] The adsorption of HTO increased slowly in the first 2 hours and basically reached equilibrium after 5 hours, with the final adsorption capacity of 47.23 mg / g.
[0081] HTO-BPA not only has a higher final adsorption capacity than HTO, but also has a significantly faster adsorption rate. This rapid adsorption characteristic is of great significance in practical applications and can greatly improve treatment efficiency.
[0082] 8. Adsorption kinetics curves of HTO and HTO-BPA in simulated salt lake brine:
[0083] Fig. 9The adsorption kinetic curves of HTO and HTO-BPA in simulated salt lake brine (the adsorption capacity of HTO and HTO-BPA in simulated salt lake brine changes with time) are shown. The results are similar to the trend in LiOH solution, further confirming the superiority of the modified material under actual application conditions. Specifically:
[0084] In simulated salt lake brine, HTO-BPA reached adsorption equilibrium within 2 hours, and the final adsorption capacity was 39.76 mg / g.
[0085] It takes about 6 hours for HTO to reach adsorption equilibrium in simulated brine, and the final adsorption capacity is 34.12 mg / g.
[0086] Although the adsorption capacity of both materials decreased in the complex salt lake brine environment, HTO-BPA still showed a faster adsorption rate and higher adsorption capacity.
[0087] The above results show that BPA modification is not only effective in simple LiOH solution, but also performs well in complex salt lake brine environment containing multiple competing ions. This provides strong support for the potential of HTO-BPA in practical industrial lithium extraction applications.
[0088] 9. Effect of eluent acid concentration on lithium ion adsorption capacity of HTO and HTO-BPA:
[0089] Fig.10 The effect of the acid concentration of the eluent on the lithium ion adsorption capacity of HTO and HTO-BPA is shown. The results show that HTO-BPA can still maintain a high adsorption capacity at a lower acid concentration, which is beneficial to reduce material loss during the pickling process. The specific analysis is as follows:
[0090] When the acid concentration increased from 0.1 mol / L to 0.5 mol / L, the adsorption capacity of HTO dropped sharply from about 45 mg / g to less than 20 mg / g.
[0091] In contrast, the adsorption capacity of HTO-BPA decreased less within the same acid concentration range, and its adsorption capacity remained above 35 mg / g even at an acid concentration of 0.5 mol / L.
[0092] In the entire tested acid concentration range (0.1-1.0 mol / L), HTO-BPA always showed a higher adsorption capacity than HTO. This shows that BPA modification not only improves the adsorption performance of the material, but also enhances its stability in acidic environments.
[0093] When the acid concentration reaches 1.0 mol / L, the adsorption capacity of HTO-BPA remains at about 25 mg / g, while the adsorption capacity of HTO drops to about 10 mg / g. This excellent performance under high acidity conditions is crucial for the recycling and long-term stability of the material.
[0094] The practical significance of this result is that the use of HTO-BPA allows for efficient regeneration at lower acid concentrations, which can not only reduce material losses during pickling, but also reduce the environmental impact of pickling, while reducing the cost of the regeneration process.
[0095] Example 2
[0096] This embodiment proposes a surface-modified lithium ion sieve prepared by the preparation method of Example 1. The preparation method is the same as that of Example 1, so it is not repeated here.
[0097] The beneficial effects of the present invention are as follows:
[0098] The lithium ion sieve surface modified with phenylphosphinic acid provided by the present invention has significantly improved adsorption performance. Through BPA modification, the water layer on the surface of the lithium ion sieve is successfully broken, the powder aggregation is reduced, and the specific surface area of the material and the accessibility of the adsorption active sites are improved. The modified lithium ion sieve shows faster adsorption kinetics, and the maximum adsorption capacity can be reached within 1 hour, while the unmodified material needs 5 hours to approach the maximum adsorption capacity. This significant increase in adsorption rate is of great significance for improving the processing efficiency in industrial applications. The preparation method of the present invention achieves precise control of material properties by optimizing the ratio of lithium source and titanium source, regulating heat treatment conditions, and selecting appropriate pH value and BPA addition amount. The modified lithium ion sieve not only shows higher adsorption capacity, but also has good structural stability and recycling performance. The test results in simulated salt lake brine show that the modified lithium ion sieve of the present invention can still maintain excellent performance in complex practical application environments. In addition, the good adsorption capacity of the modified material at lower acid concentrations helps to reduce material loss during pickling and improves the service life and economy of the material. These characteristics make the lithium ion sieve of the present invention have broad prospects in industrial lithium extraction applications.
[0099] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A preparation method for surface modification of lithium ion sieve using phenylphosphinic acid, characterized in that: The following steps are involved: S001. preparing a lithium titanium oxide precursor; S002, mixing the precursor with phenylphosphinic acid in a buffer solution; S003. Treat the mixed materials with acid.
2. The preparation method according to claim 1, characterized in that: The process of preparing the lithium titanium oxide precursor in step S001 includes: The mixture of lithium source and titanium source is mixed with flux, ground by adding solvent, dried and then heat treated.
3. The preparation method according to claim 2, characterized in that: The lithium source is Li2CO3, the titanium source is TiO2, and the flux is LiCl.
4. The preparation method according to claim 2, characterized in that: The molar ratio of the lithium source to the titanium source is 2:
1.
5. The preparation method according to claim 2, characterized in that: The solvent is anhydrous ethanol.
6. The preparation method according to claim 2, characterized in that: The heat treatment comprises calcining at 70-90° C. for 0.6-1.5 h and then heating to 600-700° C. for 2-6 h.
7. The preparation method according to claim 1, characterized in that: The buffer solution in step S002 is a tris(hydroxymethyl)aminomethane buffer solution with a pH value of 7.5-9.
5.
8. The preparation method according to claim 1, characterized in that: In step S002, the amount of phenylphosphinic acid added is 0-50% of the mass of the precursor.
9. The preparation method according to claim 1, characterized in that: The acid treatment in step S003 uses a 0.1-0.5 mol / L acid solution at 20-30° C. for 12-36 hours.
10. A surface-modified lithium ion sieve, characterized in that: The lithium ion sieve is prepared according to the method according to any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of titanium type lithium ion sieve adsorbent
CN107243318A
Directional liquid guide composite membrane with lithium extraction function, preparation method and application
CN114225720A
PH response type lithium extraction membrane as well as preparation method and application thereof
CN115181865A
Method for preparing lithium ion sieve adsorbent particles and application
CN116328713A
Hydrophobic lithium type oxygen generation molecular sieve adsorbent as well as preparation method and application thereof
CN116474718A