Flotation separation method for copper-molybdenum ore

By adjusting the pH value and potential of the copper-molybdenum slurry, using long-chain hydrocarbon oil collectors and expanded graphite adsorbents, the low associated metal recovery rate and excessive use of agents in the copper-molybdenum ore flotation process in the existing technology are solved. The problem has achieved efficient and low-cost copper-molybdenum ore separation effect.

CN118950259AActive Publication Date: 2024-11-15CENT SOUTH UNIV +2

Patent Information

Application Number
CN202411029595.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In the existing copper-molybdenum flotation process, copper-molybdenum mixed float or molybdenum copper can be added to float to suppress pyrite, but at the same time, molybdenum ore and gold and silver minerals are inhibited, resulting in low recovery of associated metals, and traditional The sexual collector forms strong chemical adsorption on the surface of chalcopyrite, increasing the subsequent separation cost and safety and environmental pressure.

Method used

By adjusting the pH value and potential of the copper-molybdenum slurry, hydrophobic substances are generated on the surface of chalcopyrite, long-chain hydrocarbon oil collectors are used to replace polar collectors, combined with expanded graphite adsorbents, reduce the use of lime and improve selectivity The effect of desorption from the agent can avoid inhibiting molybdenumite.

Benefits of technology

It significantly improves the separation and recycling efficiency of copper and molybdenum, improves the recovery rate of associated metals, reduces the production cost, and reduces the use of lime and other chemicals. It is suitable for industrial applications, and has a simple process and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950259A_ABST
    Figure CN118950259A_ABST
Patent Text Reader

Abstract

The invention discloses a flotation separation method for copper-molybdenum ore. The method comprises the following steps that (1) copper-molybdenum raw ore is subjected to ore grinding, copper-molybdenum ore pulp is obtained, in the ore grinding process, the pH value of the copper-molybdenum ore pulp is adjusted to 7.5-9.5 by adding an ore pulp adjusting agent, and the electric potential is 200-300 mV; (2) a non-polar collecting agent and a foaming agent are added into the copper-molybdenum ore pulp for rough flotation, and flotation concentrate and flotation tailings are obtained; carrying out blank concentration on the flotation concentrate to obtain copper-molybdenum bulk concentrate; (3) the copper-molybdenum bulk concentrate and expanded graphite are mixed and ground, copper-molybdenum bulk concentrate ore pulp is obtained, and molybdenum concentrate and copper concentrate I are obtained through one-time roughing and multiple-time concentration of the copper-molybdenum bulk concentrate ore pulp; and (4) the flotation tailings are subjected to one-time roughing and multiple-time concentration, and copper concentrate II is obtained. The influence of lime on copper and molybdenum recovery can be reduced, and the flotation recovery rate of copper and molybdenum is greatly increased; and meanwhile, the use amount of a copper-molybdenum separation inhibitor can be greatly reduced, and clean and efficient flotation recovery of copper-molybdenum ore is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of mineral flotation technology and reagents, and in particular to a flotation separation method for copper-molybdenum ore, belonging to the technical field of copper-molybdenum ore separation. Background Art

[0002] As a very important rare metal and strategic reserve resource, molybdenum has good electrical conductivity, processing stability, high temperature and high strength properties. It is used in electronic product manufacturing, chemical industry, metallurgy, national defense and various fields of daily life. Copper, as a strategic metal resource, is also widely used in new energy, electrical, electronic and other fields. Porphyry copper-molybdenum ore is the main source of copper and molybdenum resources. At present, the flotation recovery of such ores mainly adopts two processes: copper-molybdenum mixed flotation-copper-molybdenum separation or molybdenum-copper and other floatable-enhanced copper flotation-copper-molybdenum separation. Lime is added as a pyrite inhibitor in copper-molybdenum mixed flotation or molybdenum-copper and other floatable operations, and Z200 polar collectors are used as copper-molybdenum collectors. Sodium sulfide or sodium hydrosulfide is added to the copper-molybdenum separation operation to remove the chalcopyrite surface, and sodium thioglycolate is added to inhibit chalcopyrite. However, in the actual production process, the process and reagent system still have the following major problems: (1) When a large amount of lime is added in the copper-molybdenum mixed flotation or equal flotation operation to inhibit pyrite, it also inhibits molybdenite and gold and silver minerals, resulting in a low recovery rate of associated metals; (2) Since polar collectors are added in the copper-molybdenum flotation process, the reagent forms a strong chemical adsorption on the surface of chalcopyrite. Therefore, in the subsequent copper-molybdenum separation operation, a large amount of sodium sulfide or sodium hydrosulfide needs to be added to ensure the effective desorption of the reagent on the chalcopyrite surface, which not only increases the cost of copper-molybdenum separation, but also brings safety and environmental protection issues and water treatment problems.

[0003] Therefore, there is an urgent need to invent a flotation separation method for copper-molybdenum ore that is clean, efficient, and has a strong sorting effect to ensure the efficient recovery and utilization of copper-molybdenum resources. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention aims to provide a flotation separation method for copper-molybdenum ore. The method can greatly improve the separation and recovery efficiency of copper and molybdenum, and the method is simple, low-cost, green and environmentally friendly, and suitable for industrial application.

[0005] In order to achieve the above technical objectives, the present invention provides a flotation separation method for copper-molybdenum ore. The method comprises the following steps:

[0006] 1) grinding the copper-molybdenum ore to obtain copper-molybdenum slurry, and adjusting the pH value of the copper-molybdenum slurry to 7.5-9.5 and the potential to 200-300 mV by adding a slurry adjuster during the grinding process;

[0007] 2) adding a collector and a frother to the copper-molybdenum slurry for rough flotation to obtain a flotation concentrate and a flotation tailing; the flotation concentrate is subjected to blank concentration to obtain a copper-molybdenum mixed concentrate;

[0008] 3) Mixing the copper-molybdenum mixed concentrate with expanded graphite and grinding to obtain copper-molybdenum mixed concentrate slurry; the copper-molybdenum mixed concentrate slurry is subjected to primary roughing to obtain molybdenum rough concentrate and copper rough concentrate I; the molybdenum rough concentrate is subjected to concentrating to obtain molybdenum concentrate; the copper rough concentrate is subjected to scavenging to obtain copper concentrate I;

[0009] 4) The flotation tailings are subjected to a roughing process and multiple cleaning processes to obtain copper concentrate II.

[0010] The invention first grinds the copper-molybdenum ore to separate the copper and molybdenum minerals from the gangue minerals, and then adjusts the pH value and potential of the copper-molybdenum ore mixed pulp to generate hydrophobic substances such as elemental sulfur on the surface of chalcopyrite, and hydrophilic substances such as iron hydroxide on the surface of pyrite, thereby ensuring the efficient flotation of chalcopyrite and inhibiting the floating of pyrite, thereby enhancing the flotation separation effect; secondly, in the rough flotation process, a long-chain hydrocarbon oil collector is used to replace a traditional polar collector, thereby significantly improving the selectivity and reducing the floating of pyrite, and at the same time, the hydrophobicity of the chalcopyrite surface is enhanced due to the pulp adjustment, so that the hydrocarbon oil The collector forms effective hydrophobic adsorption and hydrogen bond adsorption with the surface of pyrite, ensuring the recovery of chalcopyrite and molybdenite; thirdly, no lime is added during the rough flotation process, effectively avoiding the inhibitory effect of lime on molybdenite and gold and silver minerals, and significantly improving the recovery rate of associated metals; fourthly, since the surface of chalcopyrite in the copper-molybdenum mixed concentrate does not chemically adsorb the polar collector, it is easier to desorb later, which is beneficial to the subsequent copper-molybdenum separation operation. At the same time, the expanded graphite used in the present invention has abundant pores and active sites, and can effectively adsorb hydrocarbon oil collectors during the regrinding process of the copper-molybdenum mixed concentrate, thereby enhancing the desorption effect of the agent.

[0011] As a preferred solution, the copper-molybdenum ore is ground to a fineness of -74 μm and the pulp content is 55 to 75 wt%, more preferably 60 to 70 wt%.

[0012] As a preferred solution, the slurry conditioner includes a pH regulator and / or a redox agent.

[0013] As a preferred solution, the pH adjuster includes at least one of sodium hydroxide, potassium hydroxide, lime, sodium carbonate and sodium bicarbonate.

[0014] As a preferred solution, the redox agent includes at least one of sodium sulfide, sodium hydrosulfide, sodium pyrosulfite, and potassium persulfate.

[0015] As a preferred solution, the collector is a long-chain hydrocarbon oil collector.

[0016] As a preferred solution, the long-chain hydrocarbon oil collector includes at least one of paraffin-based oil, heavy oil, lubricating oil, engine oil, and tar.

[0017] As a preferred solution, the foaming agent includes 2# oil and / or methyl isobutyl carbinol (MIBC).

[0018] As a preferred solution, the amount of the collector added relative to the copper-molybdenum ore is 20 to 80 g / t.

[0019] As a preferred solution, the amount of the foaming agent added relative to the copper-molybdenum ore is 10 to 50 g / t.

[0020] As a preferred solution, the flotation concentrate is subjected to two blank concentrations to obtain a copper-molybdenum mixed concentrate.

[0021] As a preferred solution, the amount of expanded graphite added relative to the copper-molybdenum ore is 10-50 g / t.

[0022] As a preferred solution, the particle size of the expanded graphite is 10 to 100 μm.

[0023] As a preferred solution, the copper-molybdenum mixed concentrate is ground to a fineness of -38 μm and the pulp content accounts for 60 to 80 wt%.

[0024] As a preferred solution, sodium thioglycolate is added as a chalcopyrite inhibitor and kerosene is used as a collector during the roughing process of the copper-molybdenum mixed concentrate slurry.

[0025] As a preferred solution, the molybdenum rough concentrate is refined 2 to 5 times, and sodium thioglycolate is added as a chalcopyrite inhibitor each time.

[0026] As a preferred solution, the copper rough concentrate is scavenged 1 to 3 times, and kerosene is added as a collector during each scavenging.

[0027] As a preferred solution, during the roughing process of copper-molybdenum mixed concentrate slurry, the amount of sodium thioglycolate added to the copper-molybdenum ore is 10-50 g / t; the amount of kerosene added to the copper-molybdenum ore is 2-10 g / t.

[0028] As a preferred solution, in each selection process of the molybdenum rough concentrate, the amount of sodium thioglycolate added is 0.01 to 0.25 times the mass of sodium thioglycolate in the rough selection process of the copper-molybdenum mixed concentrate slurry.

[0029] As a preferred solution, during each scavenging process of the copper rough concentrate, the amount of kerosene added is 0.1 to 0.5 times the mass of kerosene during the roughing process of the copper-molybdenum mixed concentrate slurry.

[0030] As a preferred scheme, the roughing and cleaning process of the flotation tailings is as follows: the pH of the flotation tailings is adjusted to 10-12, and then a copper collector is added for roughing to obtain copper rough concentrate II and copper rough tailings; the copper rough concentrate II is ground and then blank cleaned to obtain copper concentrate II; the tailings obtained by scavenging the copper rough tailings are the final flotation tailings.

[0031] As a preferred solution, lime is used as a pH regulator in the roughing process of the flotation tailings, and the amount of lime added relative to the copper-molybdenum ore is 500-2000 g / t.

[0032] As a preferred solution, the copper collector includes at least one of a thiocarbamide collector, a xanthate collector, and a black drug collector.

[0033] As a preferred solution, the copper collector is added in an amount of 10 to 30 g / t relative to the copper-molybdenum ore.

[0034] As a preferred solution, the copper rough concentrate II is ground to a fineness of -38 μm, and the mineral content accounts for 70-90 wt%, and lime is added during the grinding process. The amount of lime added relative to the copper-molybdenum ore is 50-300 g / t. Adding lime can inhibit pyrite and improve flotation separation efficiency.

[0035] As a preferred solution, the copper rough concentrate II is subjected to two blank concentrations.

[0036] As a preferred solution, the copper rough tailings are scavenged twice, and copper collector is added each time. The amount of copper collector is 0.1 to 0.5 times the amount used in the roughing process of copper-molybdenum ore.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] (1) The separation and recovery efficiency of copper and molybdenum is high, among which the molybdenum recovery rate reaches more than 88%, the copper recovery rate reaches more than 90%, the molybdenum concentrate grade is increased to more than 48%, and the copper concentrate grade is increased to more than 21%.

[0039] (2) Chalcopyrite and pyrite are semiconductor minerals. By adding slurry adjusters and adjusting the pH and potential of the slurry, hydrophobic substances such as elemental sulfur are generated on the surface of chalcopyrite, while hydrophilic substances such as iron hydroxide are generated on the surface of pyrite. This not only ensures the efficient flotation of chalcopyrite, but also inhibits the flotation of pyrite, thereby enhancing the flotation separation effect.

[0040] (3) For the flotation of molybdenum, copper and other materials (rough flotation), long-chain hydrocarbon oil collectors are used instead of traditional polar collectors, which can significantly improve selectivity and reduce the floating of pyrite. At the same time, thanks to the enhanced hydrophobicity of the chalcopyrite surface brought about by the slurry adjustment, the hydrocarbon oil collector forms effective hydrophobic adsorption and hydrogen bond adsorption with the pyrite surface, ensuring the recovery of chalcopyrite and molybdenite.

[0041] (4) Molybdenum, copper and other floatable operations (rough flotation) do not require the addition of lime, which can effectively avoid the inhibitory effect of lime on molybdenite and gold and silver minerals, and significantly improve the recovery rate of associated metals.

[0042] (5) The surface of chalcopyrite in the copper-molybdenum mixed concentrate does not chemically adsorb the polar collector, and it is easier to desorb it later, which is beneficial to the subsequent copper-molybdenum separation operation.

[0043] (6) Expanded graphite has abundant pores and active sites, which can effectively adsorb hydrocarbon oil collectors during the regrinding process of copper-molybdenum mixed concentrate and enhance the desorption effect of the agent.

[0044] (7) The flotation process and reagent system eliminates the addition of sodium sulfide or sodium hydrosulfide, and significantly reduces the addition of reagents such as lime and sodium thioglycolate, which is beneficial for the ore dressing plant to control production costs and effectively protect the ecological benefits of the ore dressing plant.

[0045] (8) The separation method is simple, low-cost, environmentally friendly, and suitable for industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 1 is a process flow chart of the closed-circuit test used in the embodiment of the present invention. DETAILED DESCRIPTION

[0047] The present invention is further described below with reference to examples, but is not intended to limit the present invention.

[0048] Example 1

[0049] The copper content in the test raw material (copper-molybdenum ore) is 0.46wt%, and the molybdenum content is 0.020wt%. The results of process mineralogy research show that the main metal minerals in the sample are pyrite, chalcopyrite, bornite, and molybdenite.

[0050] The flotation separation method of a copper-molybdenum ore provided by the present invention is used to flotate and separate the ore sample, wherein the amount of material added involved is based on the copper-molybdenum ore sample, and the specific steps are as follows:

[0051] 1) First, grind the ore sample to a fineness of -74μm accounting for 65%. During the grinding process, add 200g / t of slurry adjuster sodium hydroxide to adjust the slurry pH to 8.0 and the slurry potential Eh to 250mV. After grinding, add 40g / t heavy oil as a collector and 30g / t 2# oil as a frother to carry out molybdenum and copper isofloatable roughing to obtain isofloatable rough concentrate and isofloatable tailings. The isofloatable rough concentrate is subjected to two blank concentrations to obtain a copper-molybdenum mixed concentrate.

[0052] 2) The copper-molybdenum mixed concentrate is re-grinded to a fineness of -38μm accounting for 70%, and 25g / t of expanded graphite with a particle size of 50μm is added during the re-grinding process, followed by the addition of 30g / t of sodium thioglycolate and 5g / t of kerosene for copper-molybdenum separation and roughing. The roughing concentrate is fined 4 times, and 5g / t, 3g / t, 2g / t and 1g / t of sodium thioglycolate are added in the 1st to 4th fines, respectively, and the final fines obtained are molybdenum concentrates. The roughing tailings are scavenged twice, and 2g / t of kerosene is added each time, and the final scavenged tailings are copper concentrate 1.

[0053] 3) 1000 g / t of lime is added to the iso-floatable tailings obtained in step (1), the pH value of the pulp is adjusted to 10.5, and then 20 g / t of Z-200 is added for roughing. The coarse concentrate is regrinded to a fineness of -38 μm accounting for 75%, 200 g / t of lime is added during the regrinding process, and then two blank concentrations are carried out (without adding any reagents), and the concentrated concentrate is copper concentrate 2. The rough tailings are scavenged twice, 10 g / t of Z-200 is added in the first scavenging, and 5 g / t of Z-200 is added in the second scavenging; the scavenged tailings are the final flotation tailings. The separation results are shown in Table 1.

[0054] Table 1

[0055]

[0056]

[0057] It can be seen from the results of this embodiment that the present invention can obtain a molybdenum concentrate with a molybdenum grade of 49.15%, and a molybdenum recovery rate of 88.76%; the copper grade in copper concentrate 1 is 23.89%, and the copper recovery rate is 68.39%; the copper grade in copper concentrate 2 is 17.67%, and the copper recovery rate is 21.84%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 22.01%, and the copper recovery rate is 90.23%.

[0058] Example 2

[0059] The method of Example 1 was used to separate and recover copper and molybdenum, except that lime was added as a slurry adjuster during the grinding of the raw ore, the slurry pH was adjusted to 8.5, and the slurry potential Eh was adjusted to 226 mV. The results are shown in Table 2.

[0060] Table 2

[0061]

[0062] This embodiment can obtain a molybdenum concentrate with a molybdenum grade of 50.22%, and a molybdenum recovery rate of 88.23%; the copper grade in copper concentrate 1 is 24.13%, and the copper recovery rate is 69.83%; the copper grade in copper concentrate 2 is 18.88%, and the copper recovery rate is 19.83%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 22.73%, and the copper recovery rate is 89.66%.

[0063] Example 3

[0064] The method of Example 1 was used to separate and recover copper and molybdenum, except that sodium sulfide was added as a slurry adjuster during the grinding of the raw ore, the slurry pH was adjusted to 9.0, and the slurry potential Eh was adjusted to 269 mV. The results are shown in Table 3.

[0065] Table 3

[0066]

[0067] This embodiment can obtain a molybdenum concentrate with a molybdenum grade of 48.62%, and a molybdenum recovery rate of 89.81%; the copper grade in copper concentrate 1 is 23.26%, and the copper recovery rate is 73.80%; the copper grade in copper concentrate 2 is 17.04%, and the copper recovery rate is 16.78%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 21.79%, and the copper recovery rate is 90.57%.

[0068] Example 4

[0069] The method of Example 1 was used to separate and recover copper and molybdenum, except that the iso-floatable roughing collector was a paraffin-based oil and a motor oil in a mass ratio of 1:1. The results are shown in Table 4.

[0070] Table 4

[0071]

[0072] This embodiment can obtain a molybdenum concentrate with a molybdenum grade of 48.73%, and a molybdenum recovery rate of 89.14%; the copper grade in copper concentrate 1 is 23.49%, and the copper recovery rate is 68.86%; the copper grade in copper concentrate 2 is 18.24%, and the copper recovery rate is 21.62%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 21.98%, and the copper recovery rate is 90.49%.

[0073] Example 5

[0074] The copper content in the test raw material (copper-molybdenum ore) is 0.37wt%, and the molybdenum content is 0.016wt%. The results of process mineralogy research show that the main metal minerals in the sample are pyrite, chalcopyrite, and molybdenite.

[0075] The flotation separation method of copper-molybdenum ore provided by the present invention is used to flotate and separate the ore sample, and the specific steps are as follows:

[0076] 1) First, grind the ore sample to a fineness of -74μm accounting for 70%. During the grinding process, add 100g / t sodium pyrosulfite and 150g / t sodium hydroxide as pulp adjusters to adjust the pulp pH to 7.5 and the pulp potential Eh to 279mV. After grinding, add 30g / t tar as a collector and 30g / t 2# oil as a frother to carry out molybdenum and copper isofloatable roughing to obtain isofloatable rough concentrate and isofloatable tailings. The isofloatable rough concentrate is subjected to two blank concentrations to obtain a copper-molybdenum mixed concentrate.

[0077] 2) The copper-molybdenum mixed concentrate is re-grinded to a fineness of -38μm accounting for 80%, and 40g / t of expanded graphite with a particle size of 80μm is added during the re-grinding process, followed by the addition of 20g / t of sodium thioglycolate and 8g / t of kerosene for copper-molybdenum separation and roughing. The roughing concentrate is fined 4 times, and 5g / t, 3g / t, 2g / t and 1g / t of sodium thioglycolate are added in the 1st to 4th fines, respectively, and the final fines obtained are molybdenum concentrates. The roughing tailings are scavenged twice, and 2g / t of kerosene is added each time, and the final scavenged tailings are copper concentrate 1.

[0078] 3) 1500 g / t of lime is added to the iso-floatable tailings obtained in step (1), the pH value of the pulp is adjusted to 11, and then 10 g / t of sodium ethyl xanthate is added for roughing. The coarse concentrate is re-ground to a fineness of -38 μm accounting for 85%, 300 g / t of lime is added during the re-grinding process, and then two blank concentrations are carried out, and the concentrated concentrate is copper concentrate 2. The rough tailings are scavenged twice, 5 g / t of sodium ethyl xanthate is added in the first scavenging, and 3 g / t of sodium ethyl xanthate is added in the second scavenging; the scavenged tailings are the final flotation tailings. The separation results are shown in Table 5.

[0079] Table 5

[0080]

[0081] This embodiment can obtain a molybdenum concentrate with a molybdenum grade of 48.42%, and a molybdenum recovery rate of 89.77%; the copper grade in copper concentrate 1 is 22.72%, and the copper recovery rate is 69.07%; the copper grade in copper concentrate 2 is 20.22%, and the copper recovery rate is 20.67%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 22.09%, and the copper recovery rate is 89.74%.

[0082] Example 6

[0083] The copper content in the test raw material (copper-molybdenum ore) is 0.32wt%, and the molybdenum content is 0.012wt%. The results of process mineralogy research show that the main metal minerals in the sample are pyrite, chalcopyrite, chalcocite, covellite, and molybdenite.

[0084] The flotation separation method of copper-molybdenum ore provided by the present invention is used to flotate and separate the ore sample, and the specific steps are as follows:

[0085] 1) First, grind the ore sample to a fineness of -74μm accounting for 60%. During the grinding process, add 50g / t potassium persulfate and 500g / t sodium hydrosulfide as pulp adjusters, adjust the pulp pH to 9.5, and the pulp potential Eh to 214mV. After grinding, add 50g / t of a heavy oil + lubricating oil combined collector with a mass ratio of 1:1 and 30g / t 2# oil as a frother to carry out molybdenum and copper isofloatable roughing, obtain isofloatable rough concentrate and isofloatable tailings, and perform two blank concentrations on the isofloatable rough concentrate to obtain a copper-molybdenum mixed concentrate.

[0086] 2) The copper-molybdenum mixed concentrate is re-grinded to a fineness of -38μm accounting for 65%. During the re-grinding process, 20g / t of expanded graphite with a particle size of 20μm is added, followed by 40g / t of sodium thioglycolate and 4g / t of kerosene for copper-molybdenum separation and roughing. The roughing concentrate is refined 4 times, and 5g / t, 3g / t, 2g / t and 1g / t of sodium thioglycolate are added in the 1st to 4th refinements, respectively. The final refinement is molybdenum concentrate. The roughing tailings are scavenged twice, and 2g / t of kerosene is added each time. The final scavenged tailings are copper concentrate 1.

[0087] 3) Add 2000g / t of lime to the iso-floatable tailings obtained in step (1), adjust the pH value of the pulp to 11.8, and then add 15g / t of ammonium butyl black medicine for roughing. The coarse concentrate is re-ground to a fineness of -38μm accounting for 70%, and 200g / t of lime is added during the re-grinding process, followed by two blank concentrations, and the concentrated concentrate is copper concentrate 2. The rough tailings are scavenged twice, and 7g / t of ammonium butyl black medicine is added in the first scavenging, and 3g / t of ammonium butyl black medicine is added in the second scavenging; the scavenging tailings are the final flotation tailings. The separation results are shown in Table 6.

[0088] Table 6

[0089]

[0090] This embodiment can obtain a molybdenum concentrate with a molybdenum grade of 49.03%, and a molybdenum recovery rate of 88.32%; the copper grade in copper concentrate 1 is 23.11%, and the copper recovery rate is 68.92%; the copper grade in copper concentrate 2 is 19.51%, and the copper recovery rate is 21.31%; after copper concentrate 1 and copper concentrate 2 are combined, the comprehensive copper grade is 22.14%, and the copper recovery rate is 90.24%.

[0091] Comparative Example 1

[0092] The method of Example 1 was used to separate and recover copper and molybdenum, except that no slurry conditioner was added during the grinding of the raw ore. The results are shown in Table 7.

[0093] Table 7

[0094]

[0095] Under the comparative conditions, a molybdenum concentrate with a molybdenum grade of 45.22% was obtained, and the molybdenum recovery rate was 87.96%; the copper grade in copper concentrate 1 was 16.73%, and the copper recovery rate was 60.20%; the copper grade in copper concentrate 2 was 16.89%, and the copper recovery rate was 28.19%; the combined copper grade of copper concentrate 1 and copper concentrate 2 was 16.78%, and the copper recovery rate was 88.39%. This result is due to the fact that the copper mineral flotation weakened after the removal of the slurry potential adjuster, while the pyrite flotation increased, resulting in a significant decrease in the concentrate grade and recovery rate.

[0096] Comparative Example 2

[0097] The method of Example 1 was used to separate and recover copper and molybdenum, except that the floatable collector was replaced with Z-200. The results are shown in Table 8.

[0098] Table 8

[0099]

[0100]

[0101] Under the comparative conditions, a molybdenum concentrate with a molybdenum grade of 38.22% was obtained, and the molybdenum recovery rate was 78.91%; the copper grade in copper concentrate 1 was 17.43%, and the copper recovery rate was 75.87%; the copper grade in copper concentrate 2 was 17.82%, and the copper recovery rate was 13.82%; after copper concentrate 1 and copper concentrate 2 were combined, the comprehensive copper grade was 17.49%, and the copper recovery rate was 89.70%. This result is due to the increase in pyrite flotation after the floatable collector was replaced from long-chain hydrocarbon oil to Z-200, resulting in a decrease in the grade of copper concentrate. At the same time, it caused the copper-molybdenum separation effect to deteriorate, and the mutual inclusion of molybdenum concentrate and copper concentrate 1 increased, resulting in a significant reduction in the molybdenum recovery rate.

[0102] Comparative Example 3

[0103] The method of Example 1 was used to separate and recover copper and molybdenum, except that no expanded graphite was added during regrinding of the copper-molybdenum mixed concentrate. The test results are shown in Table 9.

[0104] Table 9

[0105]

[0106] Under the comparative conditions, a molybdenum concentrate with a molybdenum grade of 35.26% was obtained, and the molybdenum recovery rate was 86.40%; the copper grade in copper concentrate 1 was 23.68%, and the copper recovery rate was 67.87%; the copper grade in copper concentrate 2 was 17.43%, and the copper recovery rate was 21.52%; after copper concentrate 1 and copper concentrate 2 were combined, the comprehensive copper grade was 21.80%, and the copper recovery rate was 89.39%. This result is due to the fact that the chalcopyrite surface reagent desorption is not thorough without the addition of expanded graphite, resulting in poor copper-molybdenum separation effect and a significant decrease in the grade of molybdenum concentrate.

[0107] Comparative Example 4

[0108] The method of Example 2 was used to separate and recover copper and molybdenum, except that 750 g / t of lime was added, the pH value of the slurry was adjusted to 9.5, and the slurry potential Eh was adjusted to 174 mV. The test results are shown in Table 10.

[0109] Table 10

[0110]

[0111] Under the comparative conditions, a molybdenum concentrate with a molybdenum grade of 48.22% was obtained, and the molybdenum recovery rate was 89.14%; the copper grade in copper concentrate 1 was 22.05%, and the copper recovery rate was 64.93%; the copper grade in copper concentrate 2 was 15.32%, and the copper recovery rate was 22.05%; the combined copper grade of copper concentrate 1 and copper concentrate 2 was 19.84%, and the copper recovery rate was 86.98%. The result is that the slurry potential was not adjusted, resulting in a weakening of the surface hydrophobicity difference between chalcopyrite and pyrite, which reduced the grade and recovery rate of the copper concentrate.

Claims

1. A flotation separation method for copper-molybdenum ore, characterized in that: The following steps are involved: 1) grinding the copper-molybdenum ore to obtain copper-molybdenum slurry, and adjusting the pH value of the copper-molybdenum slurry to 7.5-9.5 and the potential to 200-300 mV by adding a slurry adjuster during the grinding process; 2) adding a collector and a frother to the copper-molybdenum slurry for rough flotation to obtain a flotation concentrate and a flotation tailing; the flotation concentrate is subjected to blank concentration to obtain a copper-molybdenum mixed concentrate; 3) Mixing the copper-molybdenum mixed concentrate with expanded graphite and grinding to obtain copper-molybdenum mixed concentrate slurry; the copper-molybdenum mixed concentrate slurry is subjected to primary roughing to obtain molybdenum rough concentrate and copper rough concentrate I; the molybdenum rough concentrate is subjected to concentrating to obtain molybdenum concentrate; the copper rough concentrate is subjected to scavenging to obtain copper concentrate I; 4) The flotation tailings are subjected to a roughing process and multiple cleaning processes to obtain copper concentrate II.

2. The flotation separation method of a copper-molybdenum ore according to claim 1, characterized in that: The copper-molybdenum ore is ground to a fineness of -74 μm and the slurry content is 55-75wt%.

3. A flotation separation method for copper-molybdenum ore according to claim 1 or 2, characterized in that: The slurry conditioner includes a pH regulator and / or a redox agent.

4. The flotation separation method of a copper-molybdenum ore according to claim 3, characterized in that: The pH adjuster includes at least one of sodium hydroxide, potassium hydroxide, lime, sodium carbonate, and sodium bicarbonate; the redox agent includes at least one of sodium sulfide, sodium hydrosulfide, sodium pyrosulfite, and potassium persulfate.

5. The flotation separation method of a copper-molybdenum ore according to claim 1, characterized in that: The collector is a long-chain hydrocarbon oil collector; the long-chain hydrocarbon oil collector includes at least one of paraffin-based oil, heavy oil, lubricating oil, engine oil, and tar; The foaming agent includes 2# oil and / or methyl isobutyl carbinol; The amount of the collector added relative to the copper-molybdenum ore is 20-80 g / t; The amount of the foaming agent added relative to the copper-molybdenum ore is 10 to 50 g / t.

6. The flotation separation method of a copper-molybdenum ore according to claim 1, characterized in that: The amount of expanded graphite added relative to the copper-molybdenum ore is 10-50 g / t; the copper-molybdenum mixed concentrate is ground to a fineness of -38 μm and the content of the slurry is 60-80 wt%.

7. A flotation separation method for copper-molybdenum ore according to claim 1 or 6, characterized in that: In the roughing process of the copper-molybdenum mixed concentrate slurry, sodium thioglycolate is added as a chalcopyrite inhibitor and kerosene is used as a collector; The molybdenum rough concentrate is selected 2 to 5 times, and sodium thioglycolate is added as a chalcopyrite inhibitor each time; the copper rough concentrate is scavenged 1 to 3 times, and kerosene is added as a collector each time.

8. The flotation separation method of a copper-molybdenum ore according to claim 7, characterized in that: In the roughing process of copper-molybdenum mixed concentrate slurry, the addition amount of sodium thioglycolate relative to the copper-molybdenum ore is 10-50g / t; the addition amount of kerosene relative to the copper-molybdenum ore is 2-10g / t; During each selection process of the molybdenum rough concentrate, the amount of sodium thioglycolate added is 0.01 to 0.25 times the mass of sodium thioglycolate in the rough selection process of the copper-molybdenum mixed concentrate slurry; During each scavenging process of the copper rough concentrate, the amount of kerosene added is 0.1 to 0.5 times the mass of kerosene during the roughing process of the copper-molybdenum mixed concentrate slurry.

9. The flotation separation method of a copper-molybdenum ore according to claim 1, characterized in that: The roughing and concentrating process of the flotation tailings is as follows: adjusting the pH of the flotation tailings to 10-12 and then adding a copper collector for roughing to obtain a copper rough concentrate II; grinding the copper rough concentrate II and then performing blank concentrating to obtain a copper concentrate II.

10. The flotation separation method of a copper-molybdenum ore according to claim 9, characterized in that: The copper collector comprises at least one of a thiocarbamide collector, a xanthate collector, and a black medicine collector; and the copper collector is added in an amount of 10 to 30 g / t relative to the copper-molybdenum ore.

Citation Information

Patent Citations

  • Combined collector for floatation of porphyry copper-molybdenum mine and floatation method thereof

    CN101844107A

  • Beneficiation method for low-grade mixed copper ore containing molybdenum

    CN105435953A

  • Porphyry copper-molybdenum ore collector, and preparation method and application thereof

    CN110369142A

  • Method for recovering copper and molybdenum from mud-containing low-grade micro-fine particle embedded copper and molybdenum ore

    CN116673120A

Cited By

  • Sulfur suppression flotation method for mixed sulfur concentrate in low dissolved oxygen environment

    CN119819494A

  • A sulfur suppression flotation method for mixed sulfur concentrate in a low dissolved oxygen environment

    CN119819494B

  • Flotation inhibitor for separating chalcopyrite and molybdenite and beneficiation method for chalcopyrite and molybdenite

    CN120460147A

  • Flotation depressant for separating chalcopyrite and molybdenite, and chalcopyrite and molybdenite beneficiation method

    CN120460147B

  • Regulator for flotation of porphyry type copper-molybdenum ore and use method of regulator

    CN122209579A