Brown coal treatment method based on pre-argillization desliming

Through pre-sludge desludge treatment, the problems of poor flotation selectivity and high chemical consumption of lignite are solved, the quality of refined coal and sorting efficiency are improved, and the cost is reduced.

CN118950266AActive Publication Date: 2024-11-15CHINA UNIV OF MINING & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411242384.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-15
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The problems of poor flotation selectivity, poor floating ability, severe fine sludge pollution, large chemical consumption and high flotation cost.

Method used

Using the lignite treatment method based on pre-sludge desludge, the fine-grained coal sludge and coarse-grained coal are separated by mixing lignite with water, and the ganglite components are removed in subsequent flotation to reduce high ash fine The entrainment behavior of mud improves the quality of refined coal and flotation selectivity, and reduces the consumption of agents.

Benefits of technology

It improves the selectivity of flotation, improves the quality of refined coal, saves sorting costs, reduces the consumption of flotation agents, and achieves efficient sorting effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950266A_ABST
    Figure CN118950266A_ABST
Patent Text Reader

Abstract

The invention discloses a lignite treatment method based on pre-argillization desliming, belongs to the technical field of lignite washing and processing, and aims to solve at least one problem of poor selectivity, poor floatability, serious fine silt pollution, high reagent consumption and high flotation cost of lignite flotation in the prior art. The method comprises the following steps: mixing a lignite raw material with water, and carrying out argillization dispersion treatment on a coal-water mixture to realize pre-argillization treatment of lignite so as to obtain argillized lignite; carrying out desliming treatment on the argillized lignite to obtain fine coal slime and coarse coal; and carrying out flotation on the coarse-grained coal to obtain flotation clean coal and flotation tailings so as to finish the treatment of the lignite. The method can be used for lignite flotation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lignite washing and processing, and in particular relates to a lignite processing method based on pre-slime desliming. Background Art

[0002] Lignite has the characteristics of high water content, high ash content and low calorific value, and flotation is an effective means of processing it.

[0003] However, due to the low degree of metamorphism of lignite, it contains a large number of oxygen-containing functional groups such as carboxyl and hydroxyl groups on its surface, has poor hydrophobicity and well-developed porosity, resulting in poor conventional flotation separation effect and high reagent consumption. The clay mineral components in lignite are muddied to form high-ash fine mud, and serious fine mud covering and entrainment behavior occurs during the flotation process, reducing the flotation selectivity and contaminating the clean coal. Fine mud covering and entrainment behavior are important reasons for the low recovery rate of lignite combustible bodies.

[0004] In addition, surface modification, ultrasonic cleaning and other methods can appropriately enhance the hydrophobicity of the lignite surface, remove high-ash fine mud, and enhance the flotation effect. However, the effect is not good and the energy consumption is high. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a lignite processing method based on pre-slime desliming to solve at least one of the problems of poor selectivity, poor floatability, serious fine mud pollution, high reagent consumption and high flotation cost in the prior art of lignite flotation.

[0006] The purpose of the present invention is mainly achieved through the following technical solutions.

[0007] The present invention provides a lignite processing method based on pre-slime desliming, comprising the following steps:

[0008] Step 1: After mixing the lignite raw material with water, the coal-water mixture is subjected to mud-dispersing treatment to achieve pre-mud treatment of the lignite to obtain mud-dispersed lignite;

[0009] Step 2: desludging the muddy lignite to obtain fine coal slime and coarse coal;

[0010] Step 3: Float the coarse coal to obtain floatation clean coal and floatation tailings to complete the processing of lignite.

[0011] Furthermore, the mass ratio of the lignite raw material to water is 1:4-6.

[0012] Furthermore, before step 1, the following steps are also included:

[0013] The mined lignite is naturally dried and then crushed to obtain lignite raw materials.

[0014] Furthermore, the following steps are included between step 1 and step 2:

[0015] The particle size analysis of muddy lignite is carried out to obtain the particle size composition of muddy lignite.

[0016] Further, step 3 includes the following steps:

[0017] Step 31: adding coarse coal and water into a flotation tank for mixing and wetting to obtain flotation pulp;

[0018] Step 32: adding a collector to the flotation slurry and stirring the mixture thoroughly;

[0019] Step 33: adding a frother to the flotation slurry containing a collector and stirring the mixture thoroughly;

[0020] Step 34: introducing flotation gas into the flotation tank, and performing frothing after aeration to obtain flotation clean coal and flotation tail coal.

[0021] Furthermore, in step 31, the concentration of the flotation pulp is 60-100 g / L.

[0022] Furthermore, in step 32, the amount of collector used per ton of coarse coal is 1.0-2.0 kg.

[0023] Furthermore, in step 33, the amount of foaming agent used per ton of coarse coal is 0.2-0.6 kg.

[0024] Furthermore, in step 32, the collector includes sodium oleate solution and metal salt solution, and the molar ratio of oleate ions to metal ions is 2:1 to 1:2.

[0025] Furthermore, the heavy metal ions in the metal salt solution are divalent metal ions or trivalent metal ions.

[0026] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects.

[0027] The lignite processing method based on pre-mudding and demudding provided by the present invention does not involve complicated processes, has low investment, high sorting efficiency and obvious economic benefits. On the one hand, the lignite raw material is pre-mudified by fully considering the difference in the mud properties of useful components and gangue minerals in the lignite raw material, and the high-ash fine mud is hydrated into fine coal mud, which is separated from the coarse coal. The gangue components are further removed by subsequent flotation, which can effectively reduce the covering and entrainment behavior of the high-ash fine mud during the flotation process, avoid clean coal pollution and underflow fines, thereby greatly increasing the flotation selectivity, improving the quality of clean coal, and saving sorting costs; on the other hand, the mudification phenomenon mainly occurs on the surface of the lignite raw material particles, making the surface of the lignite raw material particles smooth, reducing the number of hydrophilic sites and pores, thereby improving the surface hydrophobicity of the lignite raw material particles, promoting the spreading of collector molecules on the coal surface, thereby reducing the consumption of flotation reagents.

[0028] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the embodiments of the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0030] Figure 1 A flow chart of a lignite processing method based on pre-slime desliming provided by the present invention;

[0031] Figure 2 A schematic diagram of the structure of a mud-removing and desludging integrated device in a lignite processing method based on pre-sludging and desludging provided by the present invention;

[0032] Figure 3 A top view of a first screen plate in the lignite processing method based on pre-slime desliming provided by the present invention;

[0033] Figure 4 A schematic structural diagram of a coal-water feed pipe in the lignite processing method based on pre-slime desliming provided by the present invention.

[0034] Reference numerals:

[0035] 1-cylinder; 2-chute; 3-first mesh plate; 31-flow stabilizing net; 32-through hole; 33-slow flow plate; 4-second mesh plate; 5-agitation wheel; 51-wheel plate; 52-reinforcement hole; 6-buffer zone; 7-mudification zone; 8-demudification zone; 9-coarse coal discharge port; 10-flushing water outlet; 11-drive motor; 12-drive shaft; 13-coal-water feed pipe; 131-first pipe; 132-second pipe; 133-convex ring; 14-coal-water feed port; 15-first brush; 16-second brush; 17-rack; 18-gear; 19-L-type mounting rod; 20-fine coal slime discharge port. DETAILED DESCRIPTION

[0036] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0037] The present invention provides a lignite processing method based on pre-slime desliming, see Figure 1 , including the following steps:

[0038] Step 1: After mixing the lignite raw material with water, the coal-water mixture is subjected to mud-dispersing treatment to achieve pre-mud treatment of the lignite to obtain mud-dispersed lignite;

[0039] Step 2: desludging the muddy lignite to obtain fine coal slime and coarse coal;

[0040] Step 3: Float the coarse coal to obtain floatation clean coal and floatation tailings (including gangue, etc.), thus completing the processing of lignite.

[0041] Compared with the prior art, the lignite processing method based on pre-mudding and demudding provided by the present invention does not involve complicated processes, has low investment, high sorting efficiency, and obvious economic benefits. On the one hand, taking full account of the difference in mud properties of useful components and gangue minerals in lignite raw materials, the lignite raw materials are pre-mudified, and high-ash fine mud (for example, clay minerals) are hydrated into fine-grained coal mud, which is separated from coarse-grained coal. The gangue components are further removed by subsequent flotation, which can effectively reduce the covering and entrainment behavior of high-ash fine mud during flotation, avoid clean coal pollution and underflow fines, thereby greatly increasing flotation selectivity, improving clean coal quality, and saving sorting costs; on the other hand, the mudification phenomenon mainly occurs on the surface of lignite raw material particles, making the surface of lignite raw material particles smooth, reducing the number of hydrophilic sites and pores, thereby improving the surface hydrophobicity of lignite raw material particles, promoting the spreading of collector molecules on the coal surface, thereby reducing the consumption of flotation reagents.

[0042] In order to fully sludge the lignite raw material, illustratively, the mass ratio of the lignite raw material to water is 1:4 to 6 (eg, 1:5).

[0043] In order to further improve the flotation effect, the above step 1 also includes the following steps:

[0044] The lignite mined from the coal field is naturally dried to remove external moisture and then crushed to obtain lignite raw materials with a particle size of <0.5mm.

[0045] In practical applications, the particle size composition of muddy lignite will directly affect the selection of various process parameters in the subsequent desludging process. Therefore, the following steps are also included between the above steps 1 and 2:

[0046] The particle size analysis of muddy lignite is carried out to obtain the particle size composition of muddy lignite.

[0047] For example, the particle size of muddy lignite is usually divided into five particle size grades: 0.5-0.25 mm, 0.25-0.125 mm, 0.125-0.074 mm, 0.074-0.045 mm and -0.045 mm. At the same time, the particle size analysis also needs to analyze the specific components in each particle size grade, for example, the specific mass percentage of fine-grained coal slime, coarse-grained coal and tailings.

[0048] In order to effectively float the coarse coal, the above step 3 includes the following steps:

[0049] Step 31: Add coarse coal and water into a flotation tank for mixing and wetting to obtain flotation pulp, wherein the concentration of the flotation pulp is 60-100 g / L;

[0050] Step 32: adding a collector to the flotation slurry and stirring the mixture sufficiently, wherein the amount of the collector used for each ton of coarse coal is 1.0 to 2.0 kg;

[0051] Step 33: adding a frother to the flotation slurry containing a collector and stirring the mixture sufficiently, wherein the amount of frother used is 0.2-0.6 kg per ton of coarse coal;

[0052] Step 34: introducing flotation gas (eg, air) into the flotation tank, and performing frothing after aeration to obtain flotation clean coal and flotation tail coal.

[0053] It should be noted that the present invention uses a collector of a specific composition that is compatible with muddy lignite. Specifically, the collector includes a sodium oleate (polar collector) solution and a metal salt solution. The heavy metal ions in the metal salt solution are divalent or trivalent, and the molar ratio of oleate ions to metal ions is 2:1 to 1:2. In this way, polar collector sodium oleate and metal salt solution are used in combination, and metal ions are bonded with oxygen elements on the surface of muddy lignite to promote the adsorption of sodium oleate. Metal ions and sodium oleate first spontaneously form oleic acid complexes, and then adsorb to the coal surface, which can significantly change the chemical properties of the lignite surface and improve the surface hydrophobicity. In addition, sodium oleate and metal salt solutions are common chemical products, low in price and easy to obtain, and the amount of reagents used during flotation is small, saving reagent costs.

[0054] Exemplarily, in the above step 1, the mudification and dispersion treatment can adopt a tumbling mudding equipment, a forced stirring equipment, an autogenous grinding equipment or a semi-autogenous grinding equipment. Specifically, the mudding time of the tumbling mudding equipment is 30 to 60 minutes, the mudding time of the forced stirring equipment is 15 to 20 minutes, the stirring speed is 1500 to 2000 rpm, and the grinding time of the autogenous grinding equipment or the semi-autogenous grinding equipment is 3 to 10 minutes.

[0055] Alternatively, in the above-mentioned lignite treatment method, mudding and desludging can be carried out by using mudding and desludging integrated equipment, specifically, see Figure 2, including a coal-water feed pipe 13, a mud-forming and desludging cylinder, and a first mesh plate 3, a second mesh plate 4 and a stirring wheel 5 arranged in the mud-forming and desludging cylinder. The first mesh plate 3 and the second mesh plate 4 divide the space in the mud-forming and desludging cylinder into a buffer zone 6, a mud-forming zone 7 and a desludging zone 8 from top to bottom. The mud-forming and desludging cylinder corresponding to the buffer zone 6 is provided with a fine-grained coal discharge port 20 and a coal-water feed port 14. The coal-water feed pipe 13 is connected to the coal-water feed port 14. The stirring wheel 5 is arranged in the mud-forming zone 7. The mud-forming and desludging cylinder corresponding to the desludging zone 8 is provided with a coarse-grained coal discharge port 9 and a flushing water port 10.

[0056] During implementation, the coal-water mixture is slowly supplied into the buffer zone 6 from the coal-water feed port 14 through the coal-water feed pipe 13. Under the action of the first mesh plate 3, the flow rate of the coal slurry is further reduced; the coal slurry in the buffer zone 6 is slowly supplied into the mudification zone 7 through the gap of the first mesh plate 3, and the stirring wheel 5 rotates to stir the coal slurry, and the slurry is fully muddied by mechanical shear force; the muddied coal slurry is slowly supplied into the desludging zone 8 through the gap of the second mesh plate 4, and flushing water is supplied into the mudification zone 7 through the flushing water port 10 to flush the muddied coal slurry and separate the fine coal slime from the coarse coal. Driven by the flushing water, the fine coal slime with smaller mass is brought to the fine coal slime discharge port 20 located at the top of the mudification and desludging cylinder and discharged from the fine coal slime discharge port 20, and the coarse coal with larger mass is discharged from the coarse coal discharge port 9 located at the bottom of the mudification and desludging cylinder.

[0057] The integrated mudding and desludging equipment of this structure integrates the mudding and desludging treatment of coal slime in the inner cavity of the same mudding and desludging cylinder, and adopts the first mesh plate 3 and the second mesh plate 4 as flow stabilizers, which can control the flow velocity of the slurry, reduce the mutual influence of the buffer zone 6, the mudding zone 7 and the desludging zone 8, and realize independent and efficient operation of each area, thereby ensuring the optimization of the separation efficiency of fine-grained coal slime and coarse-grained coal; since the flow direction of the coal slurry is opposite to the flow direction of the flushing water, the upward-flowing flushing water can flush the gaps between the first mesh plate 3 and the second mesh plate 4 and the residue in the mudding and desludging cylinder, so as to avoid the fine-grained coal slime clogging the gaps between the first mesh plate 3, the gaps between the second mesh plate 4 and the mudding and desludging cylinder, thereby realizing the self-cleaning of the integrated mudding and desludging equipment, and ensuring the cleaning efficiency and the long-term stable operation of the integrated mudding and desludging equipment.

[0058] For the structures of the first mesh plate 3 and the second mesh plate 4, see Figure 3It includes a mounting ring and a flow stabilizing sheet arranged in the inner area of ​​the mounting ring. The flow stabilizing sheet is in the shape of a grid. A flow stabilizing net 31 is arranged in some grids, and the remaining grids are through holes 32. The through holes 32 can ensure that the flushing water passes smoothly and flows upward quickly to flush the coal slurry in the desludging area 8, the mudification area 7 and the buffer area 6 to ensure the desludging efficiency and effect. The flow stabilizing net 31 can properly isolate the desludging area 8, the mudification area 7 and the buffer area 6, reduce the liquid level fluctuations in the buffer area 6 and the desludging area 8, thereby reducing the influence of the disturbance generated by the rotation of the stirring wheel 5 in the mudification area 7 on the buffer area 6 and the desludging area 8.

[0059] For example, see Figure 3 The through holes 32 and the flow-stabilizing net 31 are both rectangular in shape, and a plurality of through holes 32 and a plurality of flow-stabilizing nets 31 are alternately arranged, that is, a flow-stabilizing net 31 is provided in every other mesh.

[0060] In order to further reduce the impact of the rotation of the stirring wheel 5 on the buffer zone 6 and the desludging zone 8, the first mesh plate 3 and the second mesh plate 4 further include a flow-slowing plate 33. The flow-slowing plate 33 is arranged on the side of the flow-stabilizing plate facing the mudding zone 7. From the dual perspectives of flow stabilization and smooth flushing water flow, the flow-slowing plate 33 is fixedly connected to the side of the flow-stabilizing net 31. This is because the fluctuations generated by the rotation of the stirring wheel 5 are mainly along the radial direction of the mudding and desludging cylinder. Through the setting of the flow-slowing plate 33, the fluctuations in the mudding zone 7 can be pre-stabilized, further reducing the impact of the rotation of the stirring wheel 5 on the buffer zone 6 and the desludging zone 8, ensuring the uniform distribution of the coal slurry during the flow process, and avoiding excessively fast or uneven flow rates that lead to reduced processing efficiency and poor results.

[0061] It can be understood that in order to realize the installation and rotation of the stirring wheel 5, the above-mentioned mudding and demuding integrated equipment also includes a driving motor 11 and a driving shaft 12. The stirring wheel 5 is sleeved on the driving shaft 12, and one end of the driving shaft 12 is fixedly connected to the output shaft of the driving motor 11. The driving motor 11 drives the driving shaft 12 and the stirring wheel 5 to rotate synchronously, so as to stir and mud the coal slurry in the mudding zone 7.

[0062] In order to improve the high shear forced mudding effect, the structure of the stirring wheel 5, specifically, includes a wheel plate 51 and a strengthening hole 52 opened on the wheel plate 51. Through the setting of the strengthening hole 52, bubbles can be generated during the stirring process of the coal slurry, thereby improving the high shear forced mudding effect.

[0063] In order to further improve the high shear forced mudding effect, the number of the strengthening holes 52 is multiple, and the multiple strengthening holes 52 are arranged vertically along the wheel plate 51. From top to bottom, the width of the wheel plate 51 and the area of ​​the strengthening holes 52 are gradually increased. In this way, during the rotation of the drive shaft 12, the shear force on the coal slurry is gradually increased through the gradually increasing wheel plate 51, the mixing and homogenization degree of the coal slurry is improved, and the coal slurry is ensured to be fully strongly sheared and mudded during the treatment process, thereby achieving a more efficient mudding effect.

[0064] It can be understood that in order to facilitate the desludging and discharge of coarse-grained coal, the above-mentioned desludging cylinder includes a cylinder 1 and a chute 2, the bottom of the cylinder 1 is open, the chute 2 is buckled at the bottom opening of the cylinder 1, the flushing water outlet 10 is arranged on the side wall of the chute 2, and the coarse-grained coal discharge port 9 is arranged at the bottom end of the chute 2.

[0065] Considering that the coal-water feed port will inevitably deposit too much coal slime after long-term feeding, resulting in blockage, in the prior art, the pipeline is usually removed for pipeline blockage. However, this method requires suspending the sludge and desliming treatment of the coal slime, and the process is complicated. In this embodiment, the coal-water feed pipe 13 is a telescopic branch, see Figure 4 , that is, it includes a first tube 131 and a second tube 132 connected in sequence, the first tube is located outside the mudding and demuding cylinder, the second tube 132 is located inside the mudding and demuding cylinder, the second tube 132 is sleeved on the outer wall of the first tube 131 and is slidably and sealedly connected to the first tube 131, the first tube 131 is located outside the mudding and demuding cylinder, and the second tube 132 is provided with a convex ring 133 at one end close to the first tube 131, the second tube 132 is located inside the mudding and demuding cylinder, and the convex ring 133 is located outside the mudding and demuding cylinder.

[0066] The above-mentioned mud-removing integrated equipment also includes a feed pipe cleaning member, which includes a first brush 15, a brush rod end of the first brush 15 is fixedly connected to the first tube 131, and the bristle end of the first brush 15 protrudes into the second tube 132, and the bristles of the first brush 15 are in contact with the inner wall of the second tube 132, see Figure 4 In this way, the operator pulls the convex ring 133 back and forth to make the second tube 132 move relative to the first tube 131 , and the first brush 15 can brush the inner wall of the second tube 132 .

[0067] In order to be able to brush the discharge end of the second tube 132, the above-mentioned feed tube cleaning member also includes a second brush 16, a rack 17, a gear 18 and an L-shaped mounting rod 19. One end of the rack 17 is fixedly connected to the inner wall of the mud-demudification cylinder, and the other end is suspended. The gear 18 is rotatably connected to the outer wall of the second tube 132 through a gear shaft. The gear 18 is vertically meshed with the rack 17. One end of the L-shaped mounting rod 19 is fixedly connected to the gear 18, and the other end of the L-shaped mounting rod 19 is fixedly connected to the brush rod end of the second brush 16. The bristles of the second brush 16 are in contact with the discharge end of the second tube 132. In this way, when the second tube 132 reciprocates up and down, it will drive the gear 18 to reciprocate on the rack 17, thereby driving the gear 18 to rotate and the L-shaped mounting rod 19 to swing, so that the bristles swing back and forth relative to the discharge end of the second tube 132, and the discharge end of the second tube 132 is brushed.

[0068] Example 1

[0069] The lignite processing method of this embodiment comprises the following steps:

[0070] Step a: The lignite sample is naturally dried to remove external moisture, and then crushed to less than 0.5 mm by a crusher to increase the degree of dissociation of useful components and gangue minerals. To avoid excessive crushing, each crushing is screened by a 0.5 mm vibrating screen, and the sieve-surface material is returned to the crusher for further crushing, and the sieve-surface material is sealed and collected in a sample bag;

[0071] Step b: mixing the lignite raw material obtained in step a with clean water and performing mud-dispersion treatment to obtain mud-dispersed lignite, with the stirring speed being 1500 rpm and the mud-dispersion process lasting for 10 minutes;

[0072] Step c: The mud sample was sieved by using a set of sieves, and the particle size composition of the lignite raw material and the mud lignite was compared. The proportion of the -0.045 mm particle size increased from 29.56% to 36.89%, and the ash content increased by 1.29%;

[0073] Step d: desludging the mudded lignite to obtain fine coal slime and coarse coal;

[0074] Step e: flotation of coarse coal, control the pulp concentration to 80g / L, the impeller speed to 1800r / min, the scraper speed to 42r / min, and adjust the aeration volume to 0.1m 3 / (m 2×min). Sodium oleate solution and CaCl2 solution are used as collectors, the amount of sodium oleate is fixed at 1.025kg / t, the molar ratio of calcium ion to sodium oleate is 2:1-1:2, and the foaming agent is 2-octanol, with an amount of 0.25g / t. After slurrying the coal-water mixture for 2min, the collector is added, and the foaming agent is added after stirring for 2min, and the foaming agent is added and stirred for 0.5min. After opening the inflation valve and inflating for 10s, the clean coal is scraped and collected, and the scraping time is 3min.

[0075] The particle size distribution before and after mudding of Example 1 is shown in Table 1, and the flotation index of the clean coal before and after mudding and desludging of Example 1 is shown in Table 2.

[0076] Table 1 Particle size distribution before and after mudification of Example 1

[0077]

[0078]

[0079] Table 2 Example 1 Clean coal flotation index before and after mud desludging

[0080]

[0081] Example 2

[0082] The difference between the steps of the lignite processing method of this embodiment and those of Embodiment 1 is that the metal salt solution used in flotation in step e is FeCl3 solution.

[0083] Example 2 The flotation indexes of clean coal before and after desludging are shown in Table 3.

[0084] Table 3 Example 2 Clean coal flotation index before and after mud desludging

[0085]

[0086] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A lignite treatment method based on pre-slime desliming, It is characterized in that The following steps are involved: Step 1: After mixing the lignite raw material with water, the coal-water mixture is subjected to mud-dispersing treatment to achieve pre-mud treatment of the lignite to obtain mud-dispersed lignite; Step 2: desludging the muddy lignite to obtain fine coal slime and coarse coal; Step 3: Float the coarse coal to obtain floatation clean coal and floatation tailings to complete the processing of lignite.

2. The lignite processing method based on pre-slime desliming according to claim 1, It is characterized in that The mass ratio of the lignite raw material to water is 1:4-6.

3. The lignite processing method based on pre-slime desliming according to claim 1, It is characterized in that The step 1 also includes the following steps: The mined lignite is naturally dried and then crushed to obtain lignite raw materials.

4. The lignite processing method based on pre-slime desliming according to claim 1, It is characterized in that The following steps are also included between step 1 and step 2: The particle size analysis of muddy lignite is carried out to obtain the particle size composition of muddy lignite.

5. The lignite processing method based on pre-slime desliming according to claim 1, It is characterized in that The step 3 comprises the following steps: Step 31: adding coarse coal and water into a flotation tank for mixing and wetting to obtain flotation pulp; Step 32: adding a collector to the flotation slurry and stirring the mixture thoroughly; Step 33: adding a frother to the flotation slurry containing a collector and stirring the mixture thoroughly; Step 34: introducing flotation gas into the flotation tank, and performing frothing after aeration to obtain flotation clean coal and flotation tail coal.

6. The lignite processing method based on pre-slime desliming according to claim 5, It is characterized in that In the step 31, the concentration of the flotation pulp is 60-100 g / L.

7. The lignite processing method based on pre-slime desliming according to claim 5, It is characterized in that In the step 32, the amount of collector used per ton of coarse coal is 1.0-2.0 kg.

8. The lignite processing method based on pre-slime desliming according to claim 5, It is characterized in that In the step 33, the amount of foaming agent used per ton of coarse coal is 0.2-0.6 kg.

9. The lignite processing method based on pre-slime desliming according to claim 5, It is characterized in that In step 32, the collector includes sodium oleate solution and metal salt solution, and the molar ratio of oleate ions to metal ions is 2:1 to 1:

2.

10. The lignite processing method based on pre-slime desliming according to claim 9, It is characterized in that The heavy metal ions in the metal salt solution are divalent metal ions or trivalent metal ions.

Citation Information

Patent Citations

  • Method for using collecting agent prepared from drainage oil for flotation and defluorination of iron ores

    CN102240604A

  • Process for washing and selecting high-ash, high-water easily-argillized lignite

    CN102553708A

  • Brown coal floatation method

    CN103357507A

  • Coal slime collecting agent

    CN107597446A

  • Lignite reverse flotation upgrading method

    CN111111930A