Method for separating copper and molybdenum from copper-molybdenum bulk concentrate

By using a combination of small molecule and macromolecular organic inhibitors and inorganic inhibitors in the copper-molybdenum mixed concentrate separation process, combined with multi-mean de-drug technology, the problem of high dosage of inorganic inhibitors is solved, and the efficiency of copper-molybdenum separation is improved. Reduces safety and water quality risks.

CN118950268APending Publication Date: 2024-11-15CHINA ENFI ENG CORP +1

Patent Information

Application Number
CN202411256698.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The dosage of inorganic inhibitors in the existing copper-molybdenum mixed concentrate flotation separation process is too high, which has safety hazards and water quality problems, and it is difficult to completely replace or use only a small amount of inorganic inhibitors.

Method used

The combination of small-molecular organic inhibitors and macromolecular organic inhibitors and inorganic inhibitors is adopted to combine depharmacy techniques through multiple means, including thickening, vertical friction scrubbing and resin adsorption, to work synergistically to reduce the dosage of inorganic inhibitors.

Benefits of technology

Effectively reduce the amount of inorganic inhibitors by more than 60%, reduce safety risks and water quality pollution, improve the efficiency of copper-molybdenum separation, and achieve a lower amount of inorganic inhibitors.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of mineral separation, in particular to a copper-molybdenum separation method for copper-molybdenum bulk concentrate, which comprises the following steps: performing reagent removal treatment on copper-molybdenum bulk concentrate pulp to obtain copper-molybdenum separation pulp; and adding an inorganic inhibitor, a micromolecular organic inhibitor and a macromolecular organic inhibitor into the copper-molybdenum separated ore pulp, then adding a collecting agent, carrying out roughing to obtain roughing concentrate and roughing tailings, carrying out concentration on the roughing concentrate to obtain molybdenum concentrate, and carrying out scavenging on the roughing tailings to obtain copper concentrate. The small-molecule organic inhibitor, the macromolecular organic inhibitor and the inorganic inhibitor are adopted as a combined inhibitor, and the macromolecular inhibitor and the small-molecule inhibitor have vacancy interpenetrating and synergistic effects, so that the inhibition effect on copper sulfide minerals is enhanced, the copper-molybdenum separation efficiency is improved, and the dosage of the inorganic inhibitor is reduced; the use amount of the inorganic inhibitor can be saved by more than 60% and even can reach more than 80%, and the risk caused by storage and use of a large amount of the inorganic inhibitor is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, and in particular to a method for separating copper and molybdenum from a copper-molybdenum mixed concentrate. Background Art

[0002] Porphyry copper-molybdenum deposits are an important type of copper-molybdenum ore, which accounts for a relatively large proportion of copper-molybdenum reserves. Porphyry copper-molybdenum ore mainly uses the process of copper-molybdenum mixed flotation-copper-molybdenum separation to recover copper-molybdenum resources, and the technical key of this process is the separation of copper-molybdenum mixed concentrate. At present, there are two main processes for separating copper-molybdenum mixed concentrates: magnetic separation process and flotation process. Among them, the magnetic separation process mainly utilizes the magnetic difference between chalcopyrite and molybdenite and realizes separation by controlling the magnetic field strength; the flotation process is generally based on the natural floatability of molybdenite, and the copper-molybdenum mixed concentrate slurry is first de-doped, and then a chalcopyrite inhibitor is added to separate chalcopyrite and molybdenite by suppressing copper floating molybdenum. Compared with magnetic separation, flotation is currently the main method for separating chalcopyrite and molybdenite.

[0003] At present, the public chalcopyrite inhibitors are divided into two categories: inorganic and organic. Inorganic inhibitors include sodium sulfide inhibitors, cyanide inhibitors and Knox inhibitors. Organic inhibitors mainly include thiol compounds, thiourea compounds, carboxylic acid compounds, etc. In addition to the above-mentioned organic inhibitors, a variety of new inhibitors have been developed in recent years, mainly thiocarbonyl hydrazine, thiopronin, modified polyacrylamide, polyacrylamide-allylthiourea, rhodanine 3-acetic acid, etc.

[0004] Compared with inorganic inhibitors, organic inhibitors are relatively more interfered in practical applications. Therefore, the above-mentioned organic inhibitors are mostly in the laboratory research stage, and there are no reports of large-scale industrial applications. The most widely used and most mature process in the field is to use sodium sulfide or sodium hydrosulfide as a copper sulfide mineral inhibitor. However, the biggest problem with this process is that the dosage of inorganic inhibitors (sodium sulfide or sodium hydrosulfide) is too high, and the dosage for copper-molybdenum mixed concentrate is generally 10-30kg / t. On the one hand, inorganic inhibitors such as sodium sulfide (hydrogen) are hazardous chemicals and pose safety hazards; on the other hand, the use of a large number of inorganic inhibitors brings water quality problems and affects the use of mineral processing return water. In order to reduce the use of inorganic inhibitors and improve the separation efficiency of copper and molybdenum, thiol-containing agents are currently used in combination with sodium sulfide on site, and they have certain effects, but there is still room for optimization. For example, it is not possible to completely replace or only use a small amount of inorganic inhibitors. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect of high dosage of inorganic depressants in the existing copper-molybdenum mixed concentrate flotation separation process, thereby providing a method for separating copper and molybdenum from copper-molybdenum mixed concentrate to solve the above problem.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for separating copper and molybdenum from a copper-molybdenum mixed concentrate, comprising: performing a drug removal treatment on a copper-molybdenum mixed concentrate pulp to obtain a copper-molybdenum separation pulp;

[0008] Inorganic inhibitors, small molecule organic inhibitors and large molecule organic inhibitors are added to the copper-molybdenum separation slurry, and then a collector is added for roughing to obtain roughing concentrate and roughing tailings. The roughing concentrate is finely selected to obtain molybdenum concentrate, and the roughing tailings are scavenged to obtain copper concentrate.

[0009] Preferably, the drug removal treatment includes: concentrating the copper-molybdenum mixed concentrate slurry through a thickener to remove the drug, and then entering a vertical mill for scrubbing and drug removal.

[0010] Preferably, the mass percentage concentration of the copper-molybdenum mixed concentrate slurry is 15-25%;

[0011] And / or, the mass percentage concentration of the pulp after the thickener is concentrated and de-doped is 50-60%;

[0012] And / or, the mass percentage concentration of the slurry after scrubbing and de-medicating is 15-25%.

[0013] Preferably, after scrubbing and de-doping, the slurry is further subjected to resin adsorption.

[0014] Preferably, the resin is polystyrene resin and / or polyacrylate.

[0015] Preferably, the inorganic inhibitor is sodium sulfide and / or sodium hydrosulfide;

[0016] And / or, the small molecule organic inhibitor is one or both of 1-3-dicarboxymethyl-2-methyl-2-thioisourea and (4-carboxyphenyl)thiourea;

[0017] And / or, the macromolecular organic inhibitor is acrylamide-acrylic acid-maleic anhydride copolymer;

[0018] And / or, the collector is kerosene and / or diesel.

[0019] Preferably, the amount of the inorganic inhibitor is 3-6 kg / t based on the dry weight of the feed mineral;

[0020] And / or, the total dosage of the small molecule organic inhibitor and the macromolecular organic inhibitor is 0.3-2 kg / t, preferably 0.3-1 kg / t;

[0021] and / or, the dosage ratio of the small molecule organic inhibitor to the macromolecular organic inhibitor is (8-20):1;

[0022] And / or, the amount of the collector is 50-100 g / t.

[0023] Preferably, the number of times of selection is 5-7 times;

[0024] And / or, the scanning is performed 1-3 times.

[0025] Preferably, inorganic inhibitors, small molecule organic inhibitors, and macromolecular organic inhibitors are added in each stage of the selection operation;

[0026] And / or, a collector is added in each stage of the scanning operation.

[0027] Preferably, based on the dry weight of the feed mineral, in each stage of the above-mentioned selection operation, the amount of inorganic inhibitors used does not exceed 1 kg / t, and the total amount of small molecule organic inhibitors and macromolecular organic inhibitors does not exceed 0.3 kg / t;

[0028] And / or, in each stage of the scavenging operation, the amount of collector used is 5-10 g / t.

[0029] The technical solution of the present invention has the following advantages:

[0030] 1. A method for separating copper and molybdenum from a copper-molybdenum mixed concentrate, comprising: removing the drug from the copper-molybdenum mixed concentrate pulp to obtain a copper-molybdenum separated pulp; adding an inorganic inhibitor, a small molecule organic inhibitor, and a macromolecular organic inhibitor to the copper-molybdenum separated pulp, and then adding a collector for roughing to obtain a roughing concentrate and a roughing tailing, beneficiating the roughing concentrate to obtain a molybdenum concentrate, and scavenging the roughing tailing to obtain a copper concentrate. In order to solve the problem of high inorganic inhibitor dosage in the current copper-molybdenum mixed concentrate flotation separation process, the present invention adopts a small molecule organic inhibitor + a macromolecular organic inhibitor + an inorganic inhibitor as a combined inhibitor, interspersing the macromolecular inhibitor with the small molecule inhibitor vacancy, synergistically, strengthening the inhibitory effect on copper sulfide minerals, improving the copper-molybdenum separation efficiency, and reducing the amount of inorganic inhibitors. The amount of inorganic inhibitors can be saved by more than 60%, and can even reach more than 80%, effectively reducing the risks brought by the large-scale storage and use of inorganic inhibitors.

[0031] 2. In the method for separating copper and molybdenum from a copper-molybdenum mixed concentrate provided by the present invention, multiple means are used to remove the drug in combination, that is, resin adsorption removal is added to the traditional concentration removal and re-rubbing and washing removal to further reduce the amount of inorganic inhibitors used. DETAILED DESCRIPTION

[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0033] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0034] Example 1

[0035] This embodiment provides a method for separating copper and molybdenum from a copper-molybdenum mixed concentrate. In this embodiment, the copper-molybdenum mixed concentrate contains 24.34% copper and 1.02% molybdenum. The specific steps are as follows:

[0036] (1) A copper-molybdenum mixed concentrate slurry with a mass percentage concentration of 20% is concentrated and dedoped by a thickener to obtain a thickened slurry with a mass percentage concentration of 60%, and then the thickened slurry is sent into a vertical mill for scrubbing and stirring for 5 minutes. The scrubbed slurry concentration is diluted to 20%, and then flows through an adsorption pipeline filled with polystyrene resin. The slurry after resin adsorption is a copper-molybdenum separation slurry;

[0037] (2) Add 3kg / t of sodium sulfide to the copper-molybdenum separation slurry in step (1), stir for 3 minutes, add 300g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea, 30g / t of acrylamide-acrylic acid-maleic anhydride copolymer, continue stirring for 3 minutes, add 60g / t of kerosene, stir for 2 minutes, and perform rough separation of copper and molybdenum to obtain rough concentrate and rough tailings. Continue to perform 6 rounds of cleaning operations on the rough concentrate, adding 100g / t of sodium sulfide, 20g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea, and 2g / t of acrylamide-acrylic acid-maleic anhydride copolymer in each operation. Perform 2 scavenging operations on the rough tailings, add 10g / t of kerosene in the first scavenging operation, and add 5g / t of kerosene in the second scavenging operation. Finally, a molybdenum concentrate with a molybdenum grade of 46.78% and a recovery rate of 90.32% is obtained, and the molybdenum concentrate contains 0.58% copper.

[0038] In this embodiment, the following control group was also established:

[0039] Control group 1 used only concentrated de-doping and re-rubbing de-doping, and only used sodium sulfide as an inhibitor for copper-molybdenum separation. Other conditions remained unchanged, and the total amount of sodium sulfide used to achieve similar indicators was 18kg / t.

[0040] Control group 2 adopts concentration and re-rubbing to remove the drug and increase resin adsorption, but only uses sodium sulfide as an inhibitor. Other conditions remain unchanged. The total amount of sodium sulfide used to achieve similar indicators is 14kg / t.

[0041] Control group 3 adopts concentration and then friction and washing to remove the drug and increase resin adsorption, but only uses sodium sulfide + 1-3-dicarboxymethyl-2-methyl-2-thioisourea as an inhibitor, that is, 1-3-dicarboxymethyl-2-methyl-2-thioisourea is used to replace acrylamide-acrylic acid-maleic anhydride copolymer, and other conditions remain unchanged. The total amount of sodium sulfide used to achieve similar indicators is 5kg / t.

[0042] Control group 4 adopts concentration to remove the drug, then friction and washing to remove the drug and increase resin adsorption, but only uses sodium sulfide + acrylamide-acrylic acid-maleic anhydride copolymer as an inhibitor. In this control group, if the dosage of the macromolecular agent is set to 330g / t, the dosage is too high and there is a problem of inhibiting the flotation of molybdenum, thereby failing to achieve similar indicators. Therefore, the dosage of acrylamide-acrylic acid-maleic anhydride copolymer in this control group is set to 30g / t, and other conditions remain unchanged. The total dosage of sodium sulfide to achieve similar indicators is 8kg / t.

[0043] Example 2

[0044] This embodiment provides a method for separating copper and molybdenum from a copper-molybdenum mixed concentrate. In this embodiment, the copper-molybdenum mixed concentrate contains 26.12% copper, 1.12% molybdenum, and a small amount of secondary copper, and the separation of copper and molybdenum is relatively difficult. The specific steps are as follows:

[0045] (1) A copper-molybdenum mixed concentrate slurry with a mass percentage concentration of 20% is concentrated and dedoped by a thickener to obtain a thickened slurry with a mass percentage concentration of 60%, and then the thickened slurry is sent into a vertical mill for scrubbing and stirring for 5 minutes. The scrubbed slurry concentration is diluted to 20%, and then flows through an adsorption pipeline filled with polystyrene resin. The slurry after resin adsorption is a copper-molybdenum separation slurry;

[0046] (2) Add 5kg / t of sodium sulfide to the copper-molybdenum separation slurry in step (1), stir for 3 minutes, add 400g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea, 35g / t of acrylamide-acrylic acid-maleic anhydride copolymer, continue stirring for 3 minutes, add 70g / t of kerosene, stir for 2 minutes, and perform rough separation of copper and molybdenum to obtain rough concentrate and rough tailings. Continue to perform 6 rounds of cleaning operations on the rough concentrate, adding 120g / t of sodium sulfide, 25g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea, and 3g / t of acrylamide-acrylic acid-maleic anhydride copolymer in each operation. Perform 2 scavenging operations on the rough tailings, add 10g / t of kerosene in the first scavenging operation, and add 5g / t of kerosene in the second scavenging operation. Finally, a molybdenum concentrate with a molybdenum grade of 46.34% and a recovery rate of 92.12% is obtained, and the molybdenum concentrate contains 0.63% copper.

[0047] In this embodiment, the following control group was also established:

[0048] Control group 1 used only concentrated de-doping and re-rubbing de-doping, and used sodium sulfide as an inhibitor to separate copper and molybdenum. Other conditions remained unchanged, and the total amount of sodium sulfide used to achieve similar indicators was 25kg / t.

[0049] Control group 2 adopts concentration and re-rubbing to remove the drug and increase resin adsorption, but only uses sodium sulfide as an inhibitor. Other conditions remain unchanged. The total amount of sodium sulfide used to achieve similar indicators is 18kg / t.

[0050] Control group 3 adopts concentration and then friction and washing to remove the drug and increase resin adsorption, but only uses sodium sulfide + 1-3-dicarboxymethyl-2-methyl-2-thioisourea as inhibitor, that is, 1-3-dicarboxymethyl-2-methyl-2-thioisourea is used to replace acrylamide-acrylic acid-maleic anhydride copolymer, other conditions remain unchanged, and the total amount of sodium sulfide used to achieve similar indicators is 7kg / t.

[0051] Control group 4 adopts concentration to remove the drug, then friction and washing to remove the drug and increase resin adsorption, but only uses sodium sulfide + acrylamide-acrylic acid-maleic anhydride copolymer as an inhibitor. In this control group, if the dosage of the macromolecular agent is set to 435g / t, the excessive dosage will inhibit the flotation of molybdenum and thus fail to achieve similar indicators. Therefore, the dosage of acrylamide-acrylic acid-maleic anhydride copolymer in this control group is set to 35g / t, and other conditions remain unchanged. The total dosage of sodium sulfide to achieve similar indicators is 9kg / t.

[0052] Example 3

[0053] This embodiment provides a method for separating copper and molybdenum from a copper-molybdenum mixed concentrate. In this embodiment, the copper-molybdenum mixed concentrate contains 26.12% copper, 1.12% molybdenum, and a small amount of secondary copper, and the separation of copper and molybdenum is relatively difficult. The specific steps are as follows:

[0054] (1) A copper-molybdenum mixed concentrate slurry with a mass percentage concentration of 15% is concentrated and dedoped by a thickener to obtain a thickened slurry with a mass percentage concentration of 50%, and then the thickened slurry is sent into a vertical mill for scrubbing and stirring for 5 minutes. The scrubbed slurry concentration is diluted to 15%, and then flows through an adsorption pipeline filled with polystyrene resin. The slurry after resin adsorption is a copper-molybdenum separation slurry;

[0055] (2) Add 3kg / t of sodium sulfide to the copper-molybdenum separation slurry in step (1), stir for 3min, add 700g / t of (4-carboxyphenyl) thiourea, 35g / t of acrylamide-acrylic acid-maleic anhydride copolymer, continue stirring for 3min, add 50g / t of diesel, stir for 2min, and perform rough separation of copper and molybdenum to obtain rough concentrate and rough tailings. The rough concentrate is further subjected to 7 rounds of cleaning operation, and 120g / t of sodium sulfide, 25g / t of (4-carboxyphenyl) thiourea, and 3g / t of acrylamide-acrylic acid-maleic anhydride copolymer are added to each operation. The rough tailings are subjected to 3 scavenging operations, and 10g / t of diesel is added in the first scavenging operation, and 5g / t of diesel is added in the second scavenging operation. Finally, a molybdenum concentrate with a molybdenum grade of 46.15% and a recovery rate of 91.42% is obtained, and the molybdenum concentrate contains 0.59% copper.

[0056] In this embodiment, the following control group was also established:

[0057] Control group 1 used only concentrated deagent and re-rubbing deagent, and used sodium sulfide as an inhibitor to separate copper and molybdenum. Other conditions remained unchanged, and the total amount of sodium sulfide used to achieve similar indicators was 24kg / t.

[0058] Control group 2 adopts concentration and re-rubbing to remove the drug and increase resin adsorption, but only uses sodium sulfide as an inhibitor. Other conditions remain unchanged. The total amount of sodium sulfide used to achieve similar indicators is 17.5kg / t.

[0059] Control group 3 adopts concentration and re-rubbing to remove the drug and increase resin adsorption, but only uses sodium sulfide + (4-carboxyphenyl) thiourea as an inhibitor, that is, (4-carboxyphenyl) thiourea is used to replace acrylamide-acrylic acid-maleic anhydride copolymer, other conditions remain unchanged, and the total amount of sodium sulfide used to achieve similar indicators is 7kg / t.

[0060] Control group 4 adopts concentration to remove the drug, then friction and washing to remove the drug and increase resin adsorption, but only uses sodium sulfide + acrylamide-acrylic acid-maleic anhydride copolymer as an inhibitor. In this control group, if the macromolecular agent is set to 735g / t, the dosage is too high and there is a problem of inhibiting the flotation of molybdenum, so that similar indicators cannot be achieved. Therefore, the dosage of acrylamide-acrylic acid-maleic anhydride copolymer in this control group is set to 35g / t, and other conditions remain unchanged. The total dosage of sodium sulfide to achieve similar indicators is 8.5kg / t.

[0061] Example 4

[0062] This embodiment provides a method for separating copper and molybdenum from a copper-molybdenum mixed concentrate. In this embodiment, the copper-molybdenum mixed concentrate contains 26.12% copper, 1.12% molybdenum, and a small amount of secondary copper, and the separation of copper and molybdenum is relatively difficult. The specific steps are as follows:

[0063] (1) A copper-molybdenum mixed concentrate slurry with a mass percentage concentration of 25% is concentrated and dedoped by a thickener to obtain a thickened slurry with a mass percentage concentration of 60%, and then the thickened slurry is sent into a vertical mill for scrubbing and stirring for 5 minutes. The scrubbed slurry concentration is diluted to 25%, and then flows through an adsorption pipeline filled with polystyrene resin. The slurry after resin adsorption is a copper-molybdenum separation slurry;

[0064] (2) 6 kg / t of sodium hydrosulfide is added to the copper-molybdenum separation slurry in step (1), and after stirring for 3 min, 400 g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea and 35 g / t of acrylamide-acrylic acid-maleic anhydride copolymer are added, and after continuing to stir for 3 min, 100 g / t of kerosene is added, and after stirring for 2 min, the copper-molybdenum separation roughing is performed to obtain a roughing concentrate and a roughing tailing. The roughing concentrate is further subjected to 5 rounds of selection operations, and 120 g / t of sodium hydrosulfide, 25 g / t of 1-3-dicarboxymethyl-2-methyl-2-thioisourea and 3 g / t of acrylamide-acrylic acid-maleic anhydride copolymer are added to each operation. The roughing tailing is subjected to 1 scavenging operation, and 10 g / t of kerosene is added in the first scavenging operation, and 5 g / t of kerosene is added in the second scavenging operation. Finally, a molybdenum concentrate with a molybdenum grade of 43.23% and a recovery rate of 92.78% was obtained, and the molybdenum concentrate contained 0.83% copper.

[0065] In this embodiment, the following control group was also established:

[0066] Control group 1 used only concentrated de-doping and re-rubbing de-doping, and used sodium hydrosulfide as an inhibitor to separate copper and molybdenum. Other conditions remained unchanged, and the total amount of sodium hydrosulfide used to achieve similar indicators was 22kg / t.

[0067] Control group 2 adopts concentration and re-rubbing to remove the drug and increase resin adsorption, but only uses sodium hydrosulfide as an inhibitor. Other conditions remain unchanged. The total amount of sodium hydrosulfide used to achieve similar indicators is 16kg / t.

[0068] Control group 3 adopts concentration and then friction and washing to remove the drug and increase resin adsorption, but only sodium hydrosulfide + 1-3-dicarboxymethyl-2-methyl-2-thioisourea is used as an inhibitor, that is, 1-3-dicarboxymethyl-2-methyl-2-thioisourea is used to replace acrylamide-acrylic acid-maleic anhydride copolymer, and other conditions remain unchanged. The total amount of sodium hydrosulfide used to achieve similar indicators is 8kg / t.

[0069] Control group 4 adopts concentration to remove the drug, then friction and washing to remove the drug and increase resin adsorption, but only sodium hydrosulfide + acrylamide-acrylic acid-maleic anhydride copolymer is used as an inhibitor. In this control group, if the macromolecular agent is set to 435g / t, the dosage is too high and there is a problem of inhibiting the flotation of molybdenum, so that similar indicators cannot be achieved. Therefore, the dosage of acrylamide-acrylic acid-maleic anhydride copolymer in this control group is set to 35g / t, and other conditions remain unchanged. The total dosage of sodium hydrosulfide to achieve similar indicators is 9kg / t.

[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for separating copper and molybdenum from a copper-molybdenum mixed concentrate, characterized in that: include: The copper-molybdenum mixed concentrate slurry is subjected to drug removal treatment to obtain copper-molybdenum separation slurry; Inorganic inhibitors, small molecule organic inhibitors and large molecule organic inhibitors are added to the copper-molybdenum separation slurry, and then a collector is added for roughing to obtain roughing concentrate and roughing tailings. The roughing concentrate is finely selected to obtain molybdenum concentrate, and the roughing tailings are scavenged to obtain copper concentrate.

2. The method according to claim 1, characterized in that The de-doping treatment comprises: concentrating the copper-molybdenum mixed concentrate slurry through a thickener to remove the drug, and then entering a vertical mill to scrub and remove the drug.

3. The method according to claim 2, characterized in that The mass percentage concentration of the copper-molybdenum mixed concentrate slurry is 15-25%; And / or, the mass percentage concentration of the pulp after the thickener is concentrated and de-doped is 50-60%; And / or, the mass percentage concentration of the slurry after scrubbing and de-medicating is 15-25%.

4. The method according to claim 2 or 3, characterized in that: After scrubbing and removing the drug, the slurry is further subjected to resin adsorption.

5. The method according to claim 4, characterized in that The resin is polystyrene resin and / or polyacrylate.

6. The method according to any one of claims 1 to 5, characterized in that: The inorganic inhibitor is sodium sulfide and / or sodium hydrosulfide; And / or, the small molecule organic inhibitor is one or both of 1-3-dicarboxymethyl-2-methyl-2-thioisourea and (4-carboxyphenyl)thiourea; And / or, the macromolecular organic inhibitor is acrylamide-acrylic acid-maleic anhydride copolymer; And / or, the collector is kerosene and / or diesel.

7. The method according to any one of claims 1 to 6, characterized in that: The dosage of the inorganic inhibitor is 3-6 kg / t based on the dry weight of the feed mineral; And / or, the total dosage of the small molecule organic inhibitor and the macromolecular organic inhibitor is 0.3-2 kg / t, preferably 0.3-1 kg / t; and / or, the dosage ratio of the small molecule organic inhibitor to the macromolecular organic inhibitor is (8-20):1; And / or, the amount of the collector is 50-100 g / t.

8. The method according to any one of claims 1 to 7, characterized in that: The number of times of selection is 5-7 times; And / or, the scanning is performed 1-3 times.

9. The method according to any one of claims 1 to 8, characterized in that: In each stage of the selected operation, inorganic inhibitors, small molecule organic inhibitors and macromolecular organic inhibitors are added; And / or, a collector is added in each stage of the scanning operation.

10. The method according to claim 9, characterized in that Calculated on the dry weight of the feed mineral, in each stage of the above-mentioned selection operation, the amount of inorganic inhibitors used shall not exceed 1kg / t, and the total amount of small molecule organic inhibitors and macromolecular organic inhibitors shall not exceed 0.3kg / t; And / or, in each stage of the scavenging operation, the amount of collector used is 5-10 g / t.

Citation Information

Patent Citations

  • Copper-molybdenum separating flotation method for low-grade copper-molybdenum ore

    CN106583050A

  • Interface regulation method for flotation separation of copper-molybdenum mixed concentrate

    CN110124871A

  • Flotation method for copper-nickel sulfide ore

    CN112191369A

  • Method for utilizing copper-molybdenum bulk concentrate beneficiation backwater

    CN113275129A

  • Efficient flotation separation method for talc type secondary copper-molybdenum bulk concentrate

    CN116493139A

Cited By

  • Pre-oxidation-magnetic-flotation combined beneficiation process for strengthening separation of copper-molybdenum bulk concentrate

    CN120502415A

  • A copper-molybdenum flotation separation method for copper-molybdenum mixed concentrate

    CN122746043A