Ultrahigh-barrier heat-sealable biaxially oriented film and preparation method thereof

Through the ultra-high barrier heat sealable bidirectional stretch film with a three-layer structure, the problem of non-degradable and difficult recycling of plastic packaging products in the prior art is solved, and the high-degradable materials are achieved. The improvement of barrier properties and heat sealing performance is suitable for a variety of packaging fields and conforms to environmental protection trends.

CN118952806AInactive Publication Date: 2024-11-15XIAMEN CHANGSU IND CO LTD

Patent Information

Application Number
CN202411044314.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing plastic packaging products are non-degradable, resulting in environmental pollution and are difficult to recycle after meeting barrier and heat sealing properties. They lack environmentally friendly and degradable high-barrier heat sealing materials.

Method used

Ultra-high barrier heat-sealable bidirectional stretch film with a three-layer structure, including the upper surface layer, the intermediate barrier layer and the heat-sealing layer. It uses modified high barrier polylactic acid resin and graphene and other materials to blend and bidirectional stretching through twin screws Process preparation forms a barrier layer with high density and complex structures to improve barrier and heat sealing performance.

Benefits of technology

It achieves high barrier properties and degradability, has good heat sealing properties, is suitable for a variety of packaging fields, conforms to environmental protection trends, and improves production efficiency, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118952806A_ABST
    Figure CN118952806A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrahigh-barrier heat-sealable biaxially oriented film which comprises a base material layer and a coating barrier layer, the base material layer comprises an upper surface layer, a middle barrier layer and a heat sealing layer; the upper surface layer is prepared from the following raw materials in parts by weight: 1-5 parts of anti-sticking master batch and 95-99 parts of polylactic resin; the middle barrier layer is prepared from the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic resin; the heat sealing layer is prepared from the following raw materials in parts by weight: 1 to 10 parts of compatilizer, 1 to 5 parts of functional master batch, 25 to 80 parts of polyethylene glycol terephthalate-1, 4-cyclohexanedimethanol ester and 5 to 73 parts of polylactic resin; the modified high-barrier polylactic acid resin is prepared from the following raw materials in parts by weight: 0.1-5 parts of a layered nano inorganic material, 0.1-8 parts of a coupling agent, 0.1-5 parts of a super dispersant, 0.5-25 parts of 2, 5-furandicarboxylic acid glycol ester, 1-10 parts of a compatilizer and 47-98.2 parts of polylactic acid resin. Through reasonable formula design and film layer structure design, the heat-sealable degradable film with high barrier property is obtained, can be widely applied to various packaging fields, and has a good market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of film flexible packaging, and particularly relates to an ultra-high barrier heat-sealable biaxially stretched film and a preparation method thereof. Background Art

[0002] The use of plastic packaging products has brought great convenience to people's lives and has become an indispensable packaging material for human survival and social development. However, the disposal of waste plastic packaging products is a headache. Due to the non-degradability of waste plastic products, they can only be incinerated or landfilled. However, the incineration process will produce a large amount of harmful gases, and landfilling will occupy a large amount of land, affecting crop cultivation. In addition, the occupied land cannot be restored for a long time, affecting the sustainable use of the land. Therefore, achieving the environmental friendliness and sustainable development of plastic packaging products has become one of the most attractive and challenging directions today.

[0003] At the same time, in order to meet the packaging requirements, such as to make the packaging materials have better barrier properties and heat sealing properties, it is currently a common method to use a variety of packaging materials with different material structures for composite use. Although this combination method can meet the packaging needs of different occasions, it adds difficulties to subsequent recycling after completing the packaging mission. The Chinese patent application number CN201210294382.4 discloses a low-temperature heat-seal high-barrier coating film, including a substrate and upper and lower coating layers on the upper and lower surfaces of the substrate, an upper primer layer between the substrate and the upper coating layer, and a lower primer layer between the substrate film and the lower coating layer, wherein the upper coating layer is an acrylic coating layer, and the lower coating layer is a polyvinylidene chloride (hereinafter referred to as PVDC) coating layer; wherein the acrylic coating layer is a low-temperature heat-seal layer, and the PVDC coating layer is a high-barrier layer. When sealing, the acrylic coating layer and the PVDC coating layer are heat-sealed, that is, the inner and outer overlap seals, and the heat-sealing strength can reach 3.6N / 15mm. This coated film has the advantages of low heat-sealing temperature, high heat-sealing strength, and high barrier properties, but is not degradable.

[0004] With the implementation of the "plastic ban" and the improvement of environmental protection requirements, single-material, environmentally friendly, recyclable and degradable materials have attracted much attention. Furthermore, with the improvement of people's awareness of health and hygiene, packaging films used in food packaging and other fields are required to have not only good barrier properties, but also good heat-sealing properties. Therefore, how to obtain a high-barrier heat-sealable degradable film has become a problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above problems, the present invention provides an ultra-high barrier heat-sealable biaxially stretched film and a preparation method thereof. Through reasonable formula design and film layer structure design, a film with high barrier properties and heat-sealable degradation is obtained, which can be widely used in various packaging fields and has a good market prospect.

[0006] The technical solution of the present invention is as follows:

[0007] One of the objects of the present invention is to provide an ultra-high barrier heat-sealable biaxially oriented film, comprising a substrate layer and a coating barrier layer located on the upper surface of the substrate layer;

[0008] The substrate layer is a three-layer structure, which includes an upper surface layer, an intermediate barrier layer and a heat-sealing layer from top to bottom; the upper surface layer is composed of the following raw materials in parts by weight: 1-5 parts of anti-sticking masterbatch, 95-99 parts of polylactic acid resin; the intermediate barrier layer is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer is composed of the following raw materials in parts by weight: 1-10 parts of a compatibilizer, 1-5 parts of a functional masterbatch, 25-80 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 5-73 parts of polylactic acid resin;

[0009] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 0.1-5 parts of layered nano inorganic material, 0.1-8 parts of coupling agent, 0.1-5 parts of super dispersant, 0.5-25 parts of ethylene glycol 2,5-furandicarboxylate, 1-10 parts of compatibilizer, and 47-98.2 parts of polylactic acid resin.

[0010] Furthermore, in the modified high-barrier polylactic acid resin, the layered nano inorganic material is at least one of montmorillonite, layered silicate, mica powder, and kaolin.

[0011] Furthermore, in the modified high barrier polylactic acid resin, the compatibilizer is one or a mixture of ethylene-methyl acrylate-glycidyl methacrylate random terpolymer, ethylene-acrylate-maleic anhydride copolymer, ethylene-vinyl acetate copolymer, maleic anhydride grafted ethylene-octene copolymer, ethylene-acrylic acid copolymer and glycidyl methacrylate grafted ethylene-octene copolymer.

[0012] Furthermore, the modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows:

[0013] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:(10-50), placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 200-800 r / min for 5-20 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 3000-6000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 50-80° C., and grinding and sieving;

[0014] S12: adding the layered nano inorganic material treated in step S11 and deionized water into a reaction kettle in a mass ratio of 1:5, and adding an organic treatment agent in a mass ratio of 50%-200% of the layered nano inorganic material, stirring for 1-3h in a water bath at 60-90°C, washing with deionized water after centrifugation, drying at 50-70°C, grinding through a 500-mesh sieve, and finally activating at 100-120°C for 1-5h to obtain an organic-treated layered nano inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzylammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0015] S13: putting a coupling agent, a super dispersant and an organically treated layered nano inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 300-500 r / min for 3-6 min, and adding polylactic acid resin, stirring at a high speed for 10-25 min to obtain a mixture 1;

[0016] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 3-8 minutes to obtain a mixture 2;

[0017] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 170-235° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0018] Further, the coating liquid for coating the barrier layer is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 30-50 parts of polyvinyl alcohol emulsion, 0.1-10 parts of graphene, 5-20 parts of adhesive resin, 0.1-5 parts of curing agent, 0.5-5 parts of coupling agent, and 10-64.3 parts of solvent;

[0019] The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:1.

[0020] Furthermore, the preparation process of the water-soluble coating liquid is as follows:

[0021] S21: adding a coupling agent to the graphene, stirring at a high speed of 800-1200 r / min for 5-20 min to obtain a first mixture;

[0022] S22: adding a solvent into a reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 100-300 r / min, and continuously stirring for 5-10 min until the mixture is completely dispersed, to obtain a second mixture;

[0023] S23: gradually add the first mixture obtained in step S21 to the second mixture obtained in step S22, and stir at a speed of 300-800 r / min for 10-40 min; add adhesive resin at a speed of 100-400 r / min, and continue stirring for 5-20 min; add curing agent, and stir at a speed of 200-600 r / min for 10-60 min to obtain the water-soluble coating liquid.

[0024] Furthermore, in the heat-sealing layer, the functional masterbatch is composed of the following raw materials in parts by weight: 0.5-5 parts of lubricant, 1-10 parts of opening agent, 0.5-5 parts of antioxidant and 80-98 parts of polylactic acid resin; the lubricant is one of erucamide and oleamide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide.

[0025] Furthermore, the preparation process of the functional masterbatch is: putting the lubricant, the anti-blocking agent, the antioxidant and the polylactic acid resin into a twin-screw extruder according to the set weight proportions, and performing melt extrusion, strip drawing, cooling, pelletizing and drying at 170-235° C. to obtain the functional masterbatch.

[0026] Furthermore, the thickness of the ultra-high barrier heat-sealable biaxially stretched film is 10-80 μm, wherein the thickness of the coating barrier layer is 1-4 μm; the thickness of the upper surface layer and the heat-sealing layer are both 1-3 μm; and the thickness of the middle barrier layer is 7-70 μm.

[0027] The second object of the present invention is to provide a method for preparing an ultra-high barrier heat-sealable biaxially oriented film, comprising the following steps:

[0028] Preparation of substrate layer:

[0029] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0030] S32: mixing the raw materials of the upper surface layer, the middle barrier layer and the heat-sealing layer according to a set weight ratio, and respectively extruding them through a twin-screw extruder at 170-235° C., and the melt flows out through a T-die; using a low-pressure air knife to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 100-350 μm, and the temperature of the cold drum is 10-50° C.;

[0031] S33: The thick sheet is immersed in a water tank at 20-80°C for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 90-180°C, and the stretching ratio is (3.5-5.5)*(3.5-5.5); the stretched film is subjected to heat setting treatment, wherein the setting temperature is 140-190°C, the setting time is 5-40s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 10-15Wmin / m 2 ; Cut the rolled film as required to obtain the substrate layer;

[0032] Preparation of barrier coating:

[0033] S34: placing the substrate layer obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer of the substrate layer, and after coating, sending the film into an oven at 70-120°C for drying, and after winding, placing it in a aging chamber at 40-65°C for aging for 24-72h to obtain the ultra-high barrier heat-sealable biaxially stretched film.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. In the present invention, the layered inorganic nanoparticles in the modified high-barrier polylactic acid resin are peeled off under the action of the screw shear force, and the layered structure is dispersed in the polymer film to form a large number of parallel and stacked two-dimensional thin sheets. Small molecules such as oxygen cannot directly penetrate the film and can only penetrate through the gaps between layers. Therefore, the addition of layered inorganic nanoparticles can hinder the penetration of small molecules such as oxygen, play a tortuous maze effect, which is equivalent to extending the path for the penetration of small molecules such as oxygen, and ultimately leads to a reduction in the amount of small molecules such as oxygen permeated; in addition, 2,5-furandicarboxylic acid ethylene glycol is added to the modified high-barrier polylactic acid resin of the present invention. The addition of this component, due to the asymmetry and polarity of the furan ring, enhances the rigidity of the molecular chain segments in the structure, is not easy to flip, and the mobility of the chain segments is also reduced, which blocks the diffusion of small molecules (such as O2, CO2, etc.) and improves its barrier performance. At the same time, in the aggregated structure, due to crystallization or other factors that promote the dense stacking of molecular segments, the reduction in the number of free volume pores and free volume content further hinders the dissolution and diffusion of small molecules, thereby achieving the purpose of further improving the barrier properties. Furthermore, the crystallization of furan rings contained in 2,5-furandicarboxylic acid ethylene glycol ester can increase the density of the modified high-barrier polylactic acid resin, introduce more cross-linking points and improve its crystal structure. The increase in resin density helps to form a tighter barrier layer, and the increase in cross-linking points makes the structure of the resin more complex. 2,5-furandicarboxylic acid ethylene glycol ester and layered nano-inorganic materials work together to greatly improve the barrier properties of the resin; the compatibilizer promotes the uniform dispersion of the components in the resin, forms a homogeneous system, reduces the interface defects of the resin, and further improves the barrier properties of the resin.

[0036] 2. In the present invention, the layered structure of graphene constitutes the first barrier line, the barrier performance of polyvinyl alcohol constructs the second barrier line, and an inorganic-organic dual barrier mechanism is formed between the two. Similarly, the intermediate barrier layer once again forms an inorganic-organic dual barrier mechanism. Furthermore, the barrier properties between the coating barrier layer and the intermediate barrier layer can once again form complementary advantages, a strong combination, and form a dual barrier mechanism, forming four impeccable barrier lines, which have better barrier properties than single-component barrier materials and single-layer barrier layers, and greatly improve the barrier performance of the film.

[0037] 3. The ultra-high barrier heat-sealable biaxially stretched film provided by the present invention can be degraded under natural conditions, is non-toxic, harmless and hygienic, is a green and environmentally friendly packaging material, conforms to the trend of environmental protection, and has good barrier properties and heat-seal properties, and has a wide range of uses and good performance.

[0038] 4. In the present invention, the coating barrier layer used has better barrier properties through the synergistic effect of inorganic barrier agents and organic barrier agents. The graphene sheet structure is evenly dispersed in the film through the coating liquid, which can extend the oxygen permeation path and improve the gas barrier performance. The barrier performance is not affected by temperature and humidity. At the same time, PVA itself has good barrier properties, and the addition of this component can fill the gaps between the graphene inorganic sheet structures to form a denser film, which has a better barrier effect.

[0039] 5. The present invention provides a method for preparing an ultra-high barrier heat-sealable biaxially stretched film, which has a simple production process, high production efficiency, and can be industrialized. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic diagram of the structure of an ultra-high barrier heat-sealable biaxially stretched film.

[0041] In the figure, 10 is a substrate layer; 20 is a coating barrier layer; 13 is an upper surface layer; 12 is an intermediate barrier layer; and 11 is a heat sealing layer. DETAILED DESCRIPTION

[0042] The following is in conjunction with the preferred embodiment and with reference to the attached Figure 1 , the present invention is further described. The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values; for numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed herein; the materials, reagents, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels; the experimental methods in the following examples, unless otherwise specified, are all conventional methods.

[0043] Example 1

[0044] This embodiment provides an ultra-high barrier heat-sealable biaxially stretched film, such as Figure 1 Said, comprising a substrate layer 10 and a coating barrier layer 20 located on the upper surface of the substrate layer 10;

[0045] The substrate layer 10 is a three-layer structure, which includes an upper surface layer 13, an intermediate barrier layer 12 and a heat-sealing layer 11 from top to bottom; the upper surface layer 13 is composed of the following raw materials in parts by weight: 3 parts of anti-sticking masterbatch and 97 parts of polylactic acid resin; the intermediate barrier layer 12 is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer 11 is composed of the following raw materials in parts by weight: 5 parts of compatibilizer, 3 parts of functional masterbatch, 50 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 42 parts of polylactic acid resin;

[0046] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 3 parts of layered nano inorganic materials, 3 parts of coupling agents, 1 part of super dispersant, 10 parts of ethylene glycol 2,5-furandicarboxylate, 3 parts of compatibilizers, and 80 parts of polylactic acid resin.

[0047] Furthermore, in the modified high-barrier polylactic acid resin, the layered nano inorganic material is montmorillonite, and the compatibilizer is glycidyl methacrylate grafted ethylene-octene copolymer.

[0048] Furthermore, the modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows:

[0049] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:20, placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 500 r / min for 10 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 5000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 70°C, and grinding and sieving;

[0050] S12: adding the layered nano inorganic material treated in step S11 and deionized water in a mass ratio of 1:5 to a reactor, and adding an organic treatment agent in a mass ratio of 60% of the layered nano inorganic material, stirring for 2 hours in a water bath at 70° C., washing with deionized water after centrifugation, drying at 60° C., grinding through a 500-mesh sieve, and finally activating at 110° C. for 3 hours to obtain an organic-treated layered nano inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzyl ammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0051] S13: putting a coupling agent, a super dispersant and an organically treated layered nano-inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 400 r / min for 5 min, and adding polylactic acid resin, stirring at a high speed for 15 min to obtain a mixture 1;

[0052] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 5 minutes to obtain a mixture 2;

[0053] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 200° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0054] Furthermore, the coating liquid for coating the barrier layer 20 is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 40 parts of polyvinyl alcohol emulsion, 1 part of graphene, 10 parts of adhesive resin, 2 parts of curing agent, 2 parts of coupling agent, and 45 parts of solvent;

[0055] The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:1.

[0056] Furthermore, the preparation process of the water-soluble coating liquid is as follows:

[0057] S21: adding a coupling agent to the graphene, and stirring at a high speed of 1000 r / min for 10 min to obtain a first mixture;

[0058] S22: adding a solvent into the reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 200 r / min, and continuously stirring for 6 minutes until the mixture is completely dispersed, to obtain a second mixture;

[0059] S23: gradually add the first mixture obtained in step S21 to the second mixture obtained in step S22, and stir at a speed of 500 r / min for 20 min; add adhesive resin at a speed of 300 r / min, and continue stirring for 10 min; add curing agent, and stir at a speed of 400 r / min for 30 min to obtain the water-soluble coating liquid.

[0060] Furthermore, in the heat-sealing layer 11, the functional masterbatch is composed of the following raw materials in parts by weight: 4 parts of lubricant, 8 parts of opening agent, 1 part of antioxidant and 87 parts of polylactic acid resin; the lubricant is erucic acid amide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide; the preparation process of the functional masterbatch is: the lubricant, opening agent, antioxidant and polylactic acid resin are put into a twin-screw extruder according to the set weight parts, and melt-extrude, draw, cool, extract pellets and dry at 200°C to obtain the functional masterbatch.

[0061] This embodiment also provides a method for preparing an ultra-high barrier heat-sealable biaxially stretched film, comprising the following steps:

[0062] Preparation of substrate layer 10:

[0063] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0064] S32: the raw materials of the upper surface layer 13, the middle barrier layer 12 and the heat sealing layer 11 are mixed according to a set weight ratio, and are melted and plasticized and extruded at 195° C. by a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 230 μm, and the temperature of the cold drum is 30° C.;

[0065] S33: The thick sheet is immersed in a 50°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 120°C, and the stretching ratio is 4.5*4.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 170°C, the setting time is 12s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 12Wmin / m 2 ; The rolled film is cut as required to obtain a substrate layer 10, and the thickness of the obtained substrate layer 10 is 28 μm;

[0066] Preparation of the coated barrier layer 20:

[0067] S34: placing the substrate layer 10 obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer 13 of the substrate layer 10, and after coating, sending the film into an oven at 110°C for drying, and after winding, placing it in a aging chamber at 50°C for aging for 48 hours to obtain the ultra-high barrier heat-sealable biaxially stretched film.

[0068] The thickness of the ultra-high barrier heat-sealable biaxially stretched film prepared in this embodiment is 30 μm, wherein the thickness of the coating barrier layer 20 is 2 μm; the thickness of the upper surface layer 13 and the heat-sealing layer 11 are both 1.5 μm; and the thickness of the intermediate barrier layer 12 is 25 μm.

[0069] Example 2

[0070] This embodiment provides an ultra-high barrier heat-sealable biaxially stretched film, comprising a substrate layer and a coating barrier layer located on the upper surface of the substrate layer;

[0071] The substrate layer is a three-layer structure, which includes an upper surface layer, an intermediate barrier layer and a heat-sealing layer from top to bottom; the upper surface layer is composed of the following raw materials in parts by weight: 4 parts of anti-sticking masterbatch and 96 parts of polylactic acid resin; the intermediate barrier layer is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer is composed of the following raw materials in parts by weight: 8 parts of compatibilizer, 4 parts of functional masterbatch, 60 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 28 parts of polylactic acid resin;

[0072] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 4 parts of layered nano inorganic material, 3.5 parts of coupling agent, 1.5 parts of super dispersant, 15 parts of ethylene glycol 2,5-furandicarboxylate, 4 parts of compatibilizer, and 72 parts of polylactic acid resin.

[0073] Furthermore, in the modified high barrier polylactic acid resin, the layered nano inorganic material is obtained by mixing montmorillonite and mica powder in a mass ratio of 2:1, and the compatibilizer is a random terpolymer of ethylene-methyl acrylate-glycidyl methacrylate and a copolymer of ethylene-acrylate-maleic anhydride in a mass ratio of 1:1;

[0074] Furthermore, the modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows:

[0075] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:30, placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 600 r / min for 15 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 5500 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 75°C, and grinding and sieving;

[0076] S12: adding the layered nano inorganic material treated in step S11 and deionized water into a reaction kettle in a mass ratio of 1:5, and adding an organic treatment agent in an amount of 80% of the layered nano inorganic material, stirring for 2.5 hours in a water bath at 80° C., centrifuging, washing with deionized water, drying at 65° C., grinding through a 500-mesh sieve, and finally activating at 115° C. for 4 hours to obtain an organic-treated layered nano inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzyl ammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0077] S13: putting a coupling agent, a super dispersant and an organically treated layered nano-inorganic material into a stirrer according to a set weight ratio, stirring at a speed of 450 r / min for 4 min, and adding polylactic acid resin, stirring at a high speed for 20 min to obtain a mixture 1;

[0078] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 6 minutes to obtain a mixture 2;

[0079] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 195° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0080] Furthermore, the coating liquid for coating the barrier layer is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 45 parts of polyvinyl alcohol emulsion, 2 parts of graphene, 15 parts of adhesive resin, 2.5 parts of curing agent, 3 parts of coupling agent, and 32.5 parts of solvent;

[0081] The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:1.

[0082] Furthermore, the preparation process of the water-soluble coating liquid is as follows:

[0083] S21: adding a coupling agent to the graphene, stirring at a high speed of 1100 r / min for 15 min to obtain a first mixture;

[0084] S22: adding a solvent into the reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 250 r / min, and continuously stirring for 8 min until the mixture is completely dispersed, to obtain a second mixture;

[0085] S23: gradually add the first mixture obtained in step S21 to the second mixture obtained in step S22, and stir at a speed of 600 r / min for 30 min; add adhesive resin at a speed of 350 r / min, and continue stirring for 15 min; add curing agent, and stir at a speed of 500 r / min for 40 min to obtain the water-soluble coating liquid.

[0086] Furthermore, in the heat-sealing layer, the functional masterbatch is composed of the following raw materials in parts by weight: 4 parts of lubricant, 8 parts of opening agent, 1 part of antioxidant and 87 parts of polylactic acid resin; the lubricant is erucic acid amide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide; the preparation process of the functional masterbatch is: putting the lubricant, opening agent, antioxidant and polylactic acid resin into a twin-screw extruder according to the set weight parts, and performing melt extrusion, strip drawing, cooling, pelletizing and drying at 200°C to obtain the functional masterbatch.

[0087] This embodiment also provides a method for preparing an ultra-high barrier heat-sealable biaxially stretched film, comprising the following steps:

[0088] Preparation of substrate layer:

[0089] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0090] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 200° C. through a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 250 μm, and the temperature of the cold drum is 25° C.;

[0091] S33: The thick sheet is immersed in a 55°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 125°C, and the stretching ratio is 4.8*4.8; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 168°C, the setting time is 15s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 11Wmin / m 2 ; The rolled film is cut as required to obtain a substrate layer. The thickness of the substrate layer obtained in this embodiment is 30 μm;

[0092] Preparation of barrier coating:

[0093] S34: placing the substrate layer obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer of the substrate layer, and after coating, sending the film into an oven at 115°C for drying, and after winding, placing it in a aging chamber at 45°C for aging for 72 hours to obtain the ultra-high barrier heat-sealable biaxially stretched film.

[0094] The thickness of the ultra-high barrier heat-sealable biaxially stretched film prepared in this embodiment is 30 μm, wherein the thickness of the coating barrier layer is 2.5 μm; the thickness of the upper surface layer and the heat-seal layer are both 2 μm; and the thickness of the middle barrier layer is 23.5 μm.

[0095] Example 3

[0096] This embodiment provides an ultra-high barrier heat-sealable biaxially stretched film, comprising a substrate layer and a coating barrier layer located on the upper surface of the substrate layer;

[0097] The substrate layer is a three-layer structure, which includes an upper surface layer, an intermediate barrier layer and a heat-sealing layer from top to bottom; the upper surface layer is composed of the following raw materials in parts by weight: 5 parts of anti-sticking masterbatch and 95 parts of polylactic acid resin; the intermediate barrier layer is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer is composed of the following raw materials in parts by weight: 10 parts of a compatibilizer, 5 parts of a functional masterbatch, 80 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 5 parts of polylactic acid resin;

[0098] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 5 parts of layered nano inorganic material, 8 parts of coupling agent, 5 parts of super dispersant, 25 parts of ethylene glycol 2,5-furandicarboxylate, 10 parts of compatibilizer, and 47 parts of polylactic acid resin.

[0099] Furthermore, in the modified high-barrier polylactic acid resin, the layered nano inorganic material is montmorillonite, and the compatibilizer is glycidyl methacrylate grafted ethylene-octene copolymer.

[0100] Furthermore, the modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows:

[0101] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:50, placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 800 r / min for 20 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 6000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 80°C, and grinding and sieving;

[0102] S12: Add the layered nano inorganic material treated in step S11 and deionized water in a mass ratio of 1:5 into the reactor, and add an organic treatment agent with a mass fraction of 200% of the layered nano inorganic material, stir for 1 hour in a water bath at 90°C, centrifuge and wash with deionized water - , and dried at 70°C, ground through a 500-mesh sieve, and finally activated at 120°C for 5 hours to obtain an organic-treated layered nano-inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzylammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0103] S13: putting a coupling agent, a super dispersant and an organically treated layered nano-inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 500 r / min for 6 min, and adding polylactic acid resin, stirring at a high speed for 25 min to obtain a mixture 1;

[0104] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 8 minutes to obtain a mixture 2;

[0105] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 235° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0106] Furthermore, the coating liquid for coating the barrier layer is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 50 parts of polyvinyl alcohol emulsion, 10 parts of graphene, 20 parts of adhesive resin, 5 parts of curing agent, 5 parts of coupling agent, and 10 parts of solvent;

[0107] The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:1.

[0108] Furthermore, the preparation process of the water-soluble coating liquid is as follows:

[0109] S21: adding a coupling agent to the graphene, stirring at a high speed of 1200 r / min for 20 min to obtain a first mixture;

[0110] S22: adding a solvent into the reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 300 r / min, and continuously stirring for 10 min until the mixture is completely dispersed, to obtain a second mixture;

[0111] S23: gradually add the first mixture obtained in step S21 to the second mixture obtained in step S22, and stir at a speed of 800 r / min for 40 minutes; add adhesive resin at a speed of 400 r / min, and continue stirring for 20 minutes; add curing agent, and stir at a speed of 600 r / min for 60 minutes to obtain the water-soluble coating liquid.

[0112] Furthermore, in the heat-sealing layer, the functional masterbatch is composed of the following raw materials in parts by weight: 5 parts of lubricant, 10 parts of opening agent, 5 parts of antioxidant and 80 parts of polylactic acid resin; the lubricant is oleic acid amide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide; the preparation process of the functional masterbatch is: the lubricant, opening agent, antioxidant and polylactic acid resin are put into a twin-screw extruder according to the set weight parts, and melt-extrude, draw, cool, extract pellets and dry at 235°C to obtain the functional masterbatch.

[0113] This embodiment also provides a method for preparing an ultra-high barrier heat-sealable biaxially stretched film, comprising the following steps:

[0114] Preparation of substrate layer:

[0115] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0116] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat-sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 235° C. through a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 350 μm, and the temperature of the cold drum is 50° C.;

[0117] S33: The thick sheet is immersed in a water tank at 80°C for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 180°C, and the stretching ratio is 5.5*5.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 190°C, the setting time is 40s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 15Wmin / m 2 ; The rolled film is cut as required to obtain a substrate layer. The thickness of the substrate layer obtained in this embodiment is 76 μm;

[0118] Preparation of barrier coating:

[0119] S34: placing the substrate layer obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer of the substrate layer, and after coating, sending the film into an oven at 120°C for drying, and after winding, placing it in a aging chamber at 65°C for aging for 72 hours to obtain the ultra-high barrier heat-sealable biaxially stretched film.

[0120] The thickness of the ultra-high barrier heat-sealable biaxially oriented film prepared in this embodiment is 80 μm, wherein the thickness of the coating barrier layer is 4 μm; the thickness of the upper surface layer and the heat-seal layer are both 3 μm; and the thickness of the middle barrier layer is 70 μm.

[0121] Example 4

[0122] This embodiment provides an ultra-high barrier heat-sealable biaxially stretched film, comprising a substrate layer and a coating barrier layer located on the upper surface of the substrate layer;

[0123] The substrate layer is a three-layer structure, which includes an upper surface layer, an intermediate barrier layer and a heat-sealing layer from top to bottom; the upper surface layer is composed of the following raw materials in parts by weight: 1 part of anti-sticking masterbatch and 99 parts of polylactic acid resin; the intermediate barrier layer is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer is composed of the following raw materials in parts by weight: 1 part of a compatibilizer, 1 part of a functional masterbatch, 25 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 73 parts of polylactic acid resin;

[0124] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 0.1 parts of layered nano inorganic material, 0.1 parts of coupling agent, 0.1 parts of super dispersant, 0.5 parts of ethylene glycol 2,5-furandicarboxylate, 1 part of compatibilizer, and 98.2 parts of polylactic acid resin.

[0125] Furthermore, in the modified high-barrier polylactic acid resin, the layered nano inorganic material is montmorillonite, and the compatibilizer is glycidyl methacrylate grafted ethylene-octene copolymer.

[0126] Furthermore, the modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows:

[0127] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:10, placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 200 r / min for 5 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 3000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 50°C, and grinding and sieving;

[0128] S12: Add the layered nano inorganic material treated in step S11 and deionized water in a mass ratio of 1:5 into the reactor, and add an organic treatment agent with a mass fraction of 50% of the layered nano inorganic material, stir for 1 hour in a water bath at 60°C, centrifuge and wash with deionized water -, and dried at 50°C, ground through a 500-mesh sieve, and finally activated at 100°C for 1h to obtain an organic-treated layered nano-inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzylammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0129] S13: putting a coupling agent, a super dispersant and an organically treated layered nano-inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 300 r / min for 3 min, and adding polylactic acid resin, stirring at a high speed for 10 min to obtain a mixture 1;

[0130] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 3 minutes to obtain a mixture 2;

[0131] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 170° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0132] Further, the coating liquid for coating the barrier layer is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 30 parts of polyvinyl alcohol emulsion, 0.1 parts of graphene, 5 parts of adhesive resin, 0.1 parts of curing agent, 0.5 parts of coupling agent, and 64.3 parts of solvent;

[0133] The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:1.

[0134] Furthermore, the preparation process of the water-soluble coating liquid is as follows:

[0135] S21: adding a coupling agent to the graphene, stirring at a high speed of 800 r / min for 5 min to obtain a first mixture;

[0136] S22: adding a solvent into the reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 100 r / min, and continuously stirring for 5 min until the mixture is completely dispersed, to obtain a second mixture;

[0137] S23: gradually add the first mixture obtained in step S21 to the second mixture obtained in step S22, and stir at a speed of 300 r / min for 10 min; add adhesive resin at a speed of 100 r / min, and continue stirring for 5 min; add curing agent, and stir at a speed of 200 r / min for 10 min to obtain the water-soluble coating liquid.

[0138] Furthermore, in the heat-sealing layer, the functional masterbatch is composed of the following raw materials in parts by weight: 0.5 parts of lubricant, 1 part of opening agent, 0.5 parts of antioxidant and 98 parts of polylactic acid resin; the lubricant is oleic acid amide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide; the preparation process of the functional masterbatch is: the lubricant, opening agent, antioxidant and polylactic acid resin are put into a twin-screw extruder according to the set weight parts, and melt-extrude, draw, cool, extract pellets and dry at 170°C to obtain the functional masterbatch.

[0139] This embodiment also provides a method for preparing an ultra-high barrier heat-sealable biaxially stretched film, comprising the following steps:

[0140] Preparation of substrate layer:

[0141] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0142] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 170° C. by a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 100 μm, and the temperature of the cold drum is 10° C.;

[0143] S33: The thick sheet is immersed in a 20°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 90°C, and the stretching ratio is 3.5*3.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 140°C, the setting time is 5s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 10Wmin / m 2 ; The rolled film is cut as required to obtain the substrate. The thickness of the substrate layer obtained in this embodiment is 9 μm;

[0144] Preparation of barrier coating:

[0145] S34: placing the substrate layer obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer of the substrate layer, and after coating, sending the film into a 70°C oven for drying, and after winding, placing it in a 40°C aging chamber for aging for 24 hours to obtain the ultra-high barrier heat-sealable biaxially stretched film.

[0146] The thickness of the ultra-high barrier heat-sealable biaxially stretched film prepared in this embodiment is 10 μm, wherein the thickness of the coating barrier layer is 1 μm; the thickness of the upper surface layer and the heat-seal layer are both 1 μm; and the thickness of the middle barrier layer is 7 μm.

[0147] Among them, in the modified high barrier polylactic acid resin of this embodiment, the layered nano inorganic material can also be selected from one or more of montmorillonite, layered silicate, mica powder, and kaolin; the compatibilizer can also be selected from one or more of ethylene-methyl acrylate-glycidyl methacrylate random terpolymer, ethylene-acrylate-maleic anhydride copolymer, ethylene-vinyl acetate copolymer, maleic anhydride grafted ethylene-octene copolymer, ethylene-acrylic acid copolymer and methacrylate glycidyl methacrylate grafted ethylene-octene copolymer or a mixture of several thereof.

[0148] Comparative Example 1

[0149] The difference from Example 1 is that: this comparative example does not contain a coating barrier layer, the middle barrier layer is 100 parts of polylactic acid resin, and the heat sealing layer does not contain a compatibilizer and polyethylene terephthalate-1,4-cyclohexanedimethanol;

[0150] The heat-sealing layer of this comparative example is composed of the following raw materials in parts by weight: 3 parts of functional masterbatch and 97 parts of polylactic acid resin.

[0151] The preparation method of the high barrier heat-sealable biaxially stretched film of this comparative example comprises the following steps:

[0152] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0153] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 195° C. through a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 230 μm, and the temperature of the cold drum is 30° C.;

[0154] S33: The thick sheet is immersed in a 50°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 120°C, and the stretching ratio is 4.5*4.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 170°C, the setting time is 12s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 12Wmin / m 2 ; The rolled film is cut as required to obtain the high-barrier heat-sealable biaxially stretched film. The thickness of the obtained high-barrier heat-sealable biaxially stretched film is 30 μm, the thickness of the upper surface layer and the heat-sealing layer is 1.5 μm; the thickness of the middle barrier layer is 27 μm.

[0155] Comparative Example 2

[0156] The difference from Example 1 is that this comparative example does not contain a coating barrier layer. The preparation method of the high barrier heat-sealable biaxially stretched film of this comparative example comprises the following steps:

[0157] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0158] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 195° C. through a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 230 μm, and the temperature of the cold drum is 30° C.;

[0159] S33: The thick sheet is immersed in a 50°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 120°C, and the stretching ratio is 4.5*4.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 170°C, the setting time is 12s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 12Wmin / m 2 ; The rolled film is cut as required to obtain the high-barrier heat-sealable biaxially stretched film. The thickness of the obtained high-barrier heat-sealable biaxially stretched film is 30 μm, the thickness of the upper surface layer and the heat-sealing layer is 1.5 μm; the thickness of the middle barrier layer is 27 μm.

[0160] Comparative Example 3

[0161] The difference from Example 1 is that the intermediate barrier layer of this comparative example is 100 parts of polylactic acid resin.

[0162] Comparative Example 4

[0163] The difference from Example 1 is that: in the intermediate barrier layer of this comparative example, the modified high-barrier polylactic acid resin does not contain layered nano-inorganic materials;

[0164] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 3 parts of a coupling agent, 1 part of a super dispersant, 10 parts of ethylene 2,5-furandicarboxylate, 3 parts of a compatibilizer, and 83 parts of polylactic acid resin.

[0165] In the modified high-barrier polylactic acid resin, the compatibilizer is glycidyl methacrylate grafted ethylene-octene copolymer.

[0166] The preparation process of the modified high barrier polylactic acid resin of this comparative example is:

[0167] S11: putting a coupling agent and a super dispersant into a stirrer according to the set weight proportions, stirring at a speed of 400 r / min for 5 min, and adding polylactic acid resin, stirring at a high speed for 15 min to obtain a mixture 1;

[0168] S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 5 minutes to obtain a mixture 2;

[0169] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 200° C., draw into strips, cool, pelletize and dry to obtain the modified high-barrier polylactic acid resin.

[0170] Comparative Example 5

[0171] The difference from Example 1 is that in the intermediate barrier layer of this comparative example, the modified high-barrier polylactic acid resin does not contain ethylene 2,5-furandicarboxylate;

[0172] The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 3 parts of layered nano inorganic materials, 3 parts of coupling agents, 1 part of super dispersants, 3 parts of compatibilizers, and 90 parts of polylactic acid resin.

[0173] In the modified high-barrier polylactic acid resin, the layered nano inorganic material is montmorillonite, and the compatibilizer is glycidyl methacrylate grafted ethylene-octene copolymer.

[0174] The preparation process of the modified high barrier polylactic acid resin of this comparative example is:

[0175] S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:20, placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 500 r / min for 10 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 5000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 70°C, and grinding and sieving;

[0176] S12: adding the layered nano inorganic material treated in step S11 and deionized water in a mass ratio of 1:5 to a reactor, and adding an organic treatment agent in a mass ratio of 60% of the layered nano inorganic material, stirring for 2 hours in a water bath at 70° C., washing with deionized water after centrifugation, drying at 60° C., grinding through a 500-mesh sieve, and finally activating at 110° C. for 3 hours to obtain an organic-treated layered nano inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzyl ammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1;

[0177] S13: putting a coupling agent, a super dispersant and an organically treated layered nano-inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 400 r / min for 5 min, and adding polylactic acid resin, stirring at a high speed for 15 min to obtain a mixture 1;

[0178] S14: blending the mixture 1 and the compatibilizer at high speed for 5 minutes to obtain a mixture 2;

[0179] S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 200° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

[0180] Comparative Example 6

[0181] The difference from Example 1 is that: this comparative example does not contain a coating barrier layer, and the intermediate barrier layer of this comparative example is composed of the following raw materials in parts by weight: 100 parts of polylactic acid resin;

[0182] The preparation method of the high barrier degradable biaxially oriented film of this comparative example comprises the following steps:

[0183] S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm;

[0184] S32: the raw materials of the upper surface layer, the middle barrier layer and the heat sealing layer are mixed according to a set weight ratio, and are melted and plasticized and extruded at 195° C. through a twin-screw extruder, and the melt flows out through a T-die; a low-pressure air knife is used to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 230 μm, and the temperature of the cold drum is 30° C.;

[0185] S33: The thick sheet is immersed in a 50°C water tank for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 120°C, and the stretching ratio is 4.5*4.5; the stretched film is subjected to heat setting treatment, wherein the setting temperature is 170°C, the setting time is 12s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 12Wmin / m 2 The rolled film is slit as required to obtain the substrate layer. The thickness of the obtained high barrier biodegradable biaxially oriented film is 28 μm.

[0186] Comparative Example 7

[0187] The difference from Example 1 is that the water-soluble coating liquid for coating the barrier layer in this comparative example does not contain graphene.

[0188] Comparative Example 8

[0189] The difference from Example 1 is that the heat-sealing layer of the substrate layer of this comparative example does not contain a compatibilizer and polyethylene terephthalate-1,4-cyclohexanedimethanol;

[0190] The heat-sealing layer of this comparative example is composed of the following raw materials in parts by weight: 3 parts of functional masterbatch and 97 parts of polylactic acid resin.

[0191] Implementation effect evaluation

[0192] The following is a specific test of the ultra-high barrier heat-sealable biaxially stretched films obtained in Examples 1-4 and Comparative Examples 1-8 to further illustrate the excellent effects achieved by the present invention:

[0193] Heat sealing performance test: Test according to the standard requirements of QB / T 2358 "Test method for heat sealing strength of plastic film packaging bags";

[0194] Oxygen transmission rate performance test: Tested in accordance with ASTM D3985 "Standard Test Method for Oxygen Gas Transmission Rate Through Plastic Film and Sheeting Using a Coulometric Sensor" standard requirements;

[0195] The symbol “◎” in the table indicates excellent, the symbol “○” indicates excellent, the symbol “□” indicates good, the symbol “△” indicates fair, the symbol “☆” indicates poor, the symbol “×” indicates extremely poor, and the symbol “-” indicates not tested or no testing is required and no relevant data is available.

[0196] The test results are shown in the table below:

[0197] Table 1 Test results statistics

[0198] Heat sealability Oxygen Transmission Rate Example 1 ◎ ◎ Example 2 ◎ ◎ Example 3 ◎ ◎ Example 4 ○ ○ Comparative Example 1 × × Comparative Example 2 ◎ △ Comparative Example 3 ◎ △ Comparative Example 4 ◎ □ Comparative Example 5 ◎ □ Comparative Example 6 ◎ × Comparative Example 7 ◎ □ Comparative Example 8 × ◎

[0199] It can be seen from the above table that compared with the degradable film produced by the traditional method, the ultra-high barrier heat-seal biaxially stretched film prepared by the present invention has better barrier and heat-sealing properties, and can meet the needs of the packaging market in different fields.

[0200] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. An ultra-high barrier heat-sealable biaxially oriented film, characterized in that: It includes a substrate layer and a coating barrier layer located on the upper surface of the substrate layer; The substrate layer is a three-layer structure, which includes an upper surface layer, an intermediate barrier layer and a heat-sealing layer from top to bottom; the upper surface layer is composed of the following raw materials in parts by weight: 1-5 parts of anti-sticking masterbatch, 95-99 parts of polylactic acid resin; the intermediate barrier layer is composed of the following raw materials in parts by weight: 100 parts of modified high-barrier polylactic acid resin; the heat-sealing layer is composed of the following raw materials in parts by weight: 1-10 parts of a compatibilizer, 1-5 parts of a functional masterbatch, 25-80 parts of polyethylene terephthalate-1,4-cyclohexanedimethanol ester, and 5-73 parts of polylactic acid resin; The modified high-barrier polylactic acid resin is composed of the following raw materials in parts by weight: 0.1-5 parts of layered nano inorganic material, 0.1-8 parts of coupling agent, 0.1-5 parts of super dispersant, 0.5-25 parts of ethylene glycol 2,5-furandicarboxylate, 1-10 parts of compatibilizer, and 47-98.2 parts of polylactic acid resin.

2. The ultra-high barrier heat-sealable biaxially oriented film according to claim 1, characterized in that: In the modified high-barrier polylactic acid resin, the layered nano inorganic material is at least one of montmorillonite, layered silicate, mica powder and kaolin.

3. The ultra-high barrier heat-sealable biaxially oriented film according to claim 1, characterized in that: In the modified high barrier polylactic acid resin, the compatibilizer is one or a mixture of ethylene-methyl acrylate-glycidyl methacrylate random terpolymer, ethylene-acrylate-maleic anhydride copolymer, ethylene-vinyl acetate copolymer, maleic anhydride grafted ethylene-octene copolymer, ethylene-acrylic acid copolymer and glycidyl methacrylate grafted ethylene-octene copolymer.

4. An ultra-high barrier heat-sealable biaxially oriented film according to any one of claims 1 to 3, characterized in that: The modified high-barrier polylactic acid resin is obtained by twin-screw blending modification, and the preparation process of the modified high-barrier polylactic acid resin is as follows: S11: dissolving the layered nano inorganic material in deionized water, wherein the mass ratio of deionized water to the layered nano inorganic material is 1:(10-50), placing the mixed liquid container on a shaker, shaking until the layered nano inorganic material is evenly dispersed, and centrifuging at a speed of 200-800 r / min for 5-20 min, removing the large-size particles at the bottom of the centrifuge tube, taking the upper mixed liquid, and centrifuging the upper mixed liquid at a speed of 3000-6000 r / min, then removing the supernatant, taking the layered nano inorganic material at the bottom of the centrifuge tube, drying at 50-80° C., and grinding and sieving; S12: adding the layered nano inorganic material treated in step S11 and deionized water into a reaction kettle in a mass ratio of 1:5, and adding an organic treatment agent in a mass ratio of 50%-200% of the layered nano inorganic material, stirring for 1-3h in a water bath at 60-90°C, washing with deionized water after centrifugation, drying at 50-70°C, grinding through a 500-mesh sieve, and finally activating at 100-120°C for 1-5h to obtain an organic-treated layered nano inorganic material; the organic treatment agent is obtained by mixing dioctadecylmethylbenzylammonium, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and methacrylic acid in a mass ratio of 1:1:1; S13: putting a coupling agent, a super dispersant and an organically treated layered nano inorganic material into a stirrer according to the set weight proportions, stirring at a speed of 300-500 r / min for 3-6 min, and adding polylactic acid resin, stirring at a high speed for 10-25 min to obtain a mixture 1; S14: blending the mixture 1, ethylene 2,5-furandicarboxylate and the compatibilizer at high speed for 3-8 minutes to obtain a mixture 2; S15: Put the mixture 2 into a twin-screw extruder, melt extrude at 170-235° C., draw into strips, cool, extract pellets and dry to obtain the modified high-barrier polylactic acid resin.

5. The ultra-high barrier heat-sealable biaxially oriented film according to claim 1, characterized in that: The coating liquid for coating the barrier layer is a water-soluble coating liquid, which is composed of the following raw materials in parts by weight: 30-50 parts of polyvinyl alcohol emulsion, 0.1-10 parts of graphene, 5-20 parts of adhesive resin, 0.1-5 parts of curing agent, 0.5-5 parts of coupling agent, and 10-64.3 parts of solvent; The bonding resin is a mixture of butyl methacrylate, ethylene glycol dimethacrylate and polyurethane resin in a mass ratio of 2:1:1; the curing agent is diethylmalonic acid blocked isocyanate; the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane; and the solvent is a mixture of water and isopropanol in a mass ratio of 3:

1.

6. The ultra-high barrier heat-sealable biaxially oriented film according to claim 5, characterized in that: The preparation process of the water-soluble coating liquid is as follows: S21: adding a coupling agent to the graphene, stirring at a high speed of 800-1200 r / min for 5-20 min to obtain a first mixture; S22: adding a solvent into the reaction kettle, and slowly adding the polyvinyl alcohol emulsion at a rotation speed of 100-300 r / min, and continuously stirring for 5-10 min until the mixture is completely dispersed, to obtain a second mixture; S23: gradually adding the first mixture obtained in step S21 to the second mixture obtained in step S22, and stirring at a speed of 300-800 r / min for 10-40 min; adding an adhesive resin at a speed of 100-400 r / min, and continuously stirring for 5-20 min; Add a curing agent and stir at a rotation speed of 200-600 r / min for 10-60 min to obtain the water-soluble coating liquid.

7. The ultra-high barrier heat-sealable biaxially oriented film according to claim 1, characterized in that: In the heat-sealing layer, the functional masterbatch is composed of the following raw materials in parts by weight: 0.5-5 parts of lubricant, 1-10 parts of opening agent, 0.5-5 parts of antioxidant and 80-98 parts of polylactic acid resin; the lubricant is one of erucamide and oleamide; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 2:1; the opening agent is silicon dioxide.

8. The ultra-high barrier heat-sealable biaxially oriented film according to claim 7, characterized in that: The preparation process of the functional masterbatch is as follows: lubricant, anti-blocking agent, antioxidant and polylactic acid resin are put into a twin-screw extruder according to set weight proportions, and melt extrusion, strip drawing, cooling, pelletizing and drying are performed at 170-235° C. to obtain the functional masterbatch.

9. The ultra-high barrier heat-sealable biaxially oriented film according to claim 1, characterized in that: The thickness of the ultra-high barrier heat-sealable biaxially stretched film is 10-80 μm, wherein the thickness of the coating barrier layer is 1-4 μm; the thickness of the upper surface layer and the heat-seal layer are both 1-3 μm; and the thickness of the middle barrier layer is 7-70 μm.

10. The method for preparing an ultra-high barrier heat-sealable biaxially oriented film according to any one of claims 1 to 9, characterized in that: The following steps are involved: Preparation of substrate layer: S31: Dry all raw materials and control the moisture content of the raw materials to be less than 100 ppm; S32: mixing the raw materials of the upper surface layer, the middle barrier layer and the heat-sealing layer according to a set weight ratio, and respectively extruding them through a twin-screw extruder at 170-235° C., and the melt flows out through a T-die; using a low-pressure air knife to attach the melt to a cold drum to form a thick sheet, wherein the thickness of the thick sheet is 100-350 μm, and the temperature of the cold drum is 10-50° C.; S33: The thick sheet is immersed in a water tank at 20-80°C for pretreatment, and the thick sheet is heated and then subjected to synchronous biaxial stretching, the stretching temperature is 90-180°C, and the stretching ratio is (3.5-5.5)*(3.5-5.5); the stretched film is subjected to heat setting treatment, wherein the setting temperature is 140-190°C, the setting time is 5-40s, and then the film is cooled and corona post-treated, and then rolled up, and the corona treatment power is 10-15Wmin / m 2 ; Cut the rolled film as required to obtain the substrate layer; Preparation of coating barrier layer: S34: placing the substrate layer obtained in step S33 on the unwinding shaft of the coating machine, and pouring the coating liquid into the glue tank, adjusting the coating machine parameters, coating the surface of the upper surface layer of the substrate layer, and after coating, sending the film into an oven at 70-120°C for drying, and after winding, placing it in a aging chamber at 40-65°C for aging for 24-72h to obtain the ultra-high barrier heat-sealable biaxially stretched film.

Citation Information

Patent Citations

  • High-barrier degradable biaxially oriented film and preparation method thereof

    CN112606511A

  • High-barrier heat-sealable degradable film and preparation method thereof

    CN114103377A

  • Antibacterial heat-sealable biaxially oriented polylactic acid film and preparation method thereof

    CN115771323A

  • Heat-resistant high-strength polylactic acid composite material and preparation method thereof

    CN116218168A

  • Bio-based high-barrier biaxially oriented polyester film and preparation method thereof

    CN117719230A

Cited By

  • Alumina-plated biaxially oriented polylactic acid film with high barrier property and preparation method of alumina-plated biaxially oriented polylactic acid film

    CN119590067A