Method for preparing nanocrystalline H beta molecular sieve through ammonium fluoride etching

The commercial Hβ molecular sieve was treated by ammonium fluoride etching, and the complex process and template agent problems in the existing technology were solved. A 20nm nanocrystalline Hβ molecular sieve was prepared, which improved the isomerization performance of the catalyst and the stability of the molecular sieve, and realized industrialization Production potential.

CN118954530APending Publication Date: 2024-11-15TIANJIN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410987964.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, when preparing nanocrystalline Hβ molecular sieve, the process is complicated, the use of expensive and environmentally unfriendly organic template agents is required, and the grain size of the product is large, which is not conducive to industrial scale production, and in a macromolecular environment. The reactants have high diffusion resistance and carbon slag accumulation lead to inactivation of molecular sieve.

Method used

Commercial Hβ molecular sieve is processed by ammonium fluoride etching, and nanocrystalline Hβ molecular sieve is stripped to generate nanocrystalline Hβ molecular sieve, controlling the concentration, temperature and time of the aqueous ammonium fluoride solution, forming a 20nm nanocrystalline Hβ molecular sieve to avoid secondary etching during the suction filtration process, and The supported metal-acid bifunctional catalyst was prepared by an equal volume impregnation method.

Benefits of technology

The 20nm nanocrystalline Hβ molecular sieve was prepared by simple process, controllable conditions, and no organic template agent was used, which improved the isomerization performance and product yield of the catalyst, and enhanced the stability and selectivity of the molecular sieve.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954530A_ABST
    Figure CN118954530A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a nanocrystalline H beta molecular sieve through ammonium fluoride etching. According to the method, an ammonium fluoride aqueous solution is used for etching a commercial H beta molecular sieve, desiliconization and dealumination are carried out at the same time, the nanocrystalline H beta molecular sieve is stripped and generated while internal defects among crystals are etched, and the nanocrystalline H beta molecular sieve with the particle size of 20 nm is successfully prepared by controlling the concentration, the etching temperature and the etching time of the ammonium fluoride aqueous solution. Then, an ice-water mixture is used for suction filtration under the conditions of low temperature and dilution of a large amount of water, so that secondary etching of ammonium fluoride is prevented from continuing to occur in the suction filtration process. An organic template agent which is complex in structure, high in price and unfriendly to the environment is not used, and meanwhile the method has the advantages of being simple in process, controllable in condition and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of improvement of a method for preparing a nanocrystalline Hβ molecular sieve, and relates to a method for preparing a nanocrystalline Hβ molecular sieve by etching with ammonium fluoride. Background Art

[0002] Molecular sieve is a synthetic crystalline porous aluminosilicate material with the function of screening molecules. It has attracted attention for its large specific surface area, ordered but variable microporous channels, and adjustable pH. According to statistics from the International Molecular Sieve Association, there are currently as many as 247 types of molecular sieve framework topological structures, but only 3-5 molecular sieves are actually used in the industrial field. Hβ molecular sieve is one of the molecular sieves that have been used in industry.

[0003] Compared with other industrial molecular sieves, Hβ molecular sieve has shorter channels, smaller particle size and larger pore size, which is conducive to the mutual diffusion of molecules within or between molecular sieve crystals. In addition, the hydrothermal stability of the pore wall of Hβ molecular sieve crystal is high and can be used in high-temperature water-containing environments. The special topological structure and good hydrothermal stability make Hβ molecular sieve play an extremely important role in industrial fields such as desorption, adsorption, separation, and catalytic reactions.

[0004] However, Hβ molecular sieve still has certain defects:

[0005] 1) In a macromolecular environment, the diffusion resistance of the reactants inside the molecular sieve is too large, which will cause the product to accumulate and reduce the reaction rate.

[0006] 2) During a certain reaction period, organic macromolecular reactants will produce carbon residues in the pores, blocking the small pores in the molecular sieve, thereby interfering with the main reaction to a certain extent.

[0007] 3) The further accumulation of reactant carbon residue will shield the acid active sites of the Hβ molecular sieve, resulting in coking and deactivation of the molecular sieve.

[0008] If the preparation method of Hβ molecular sieve is adjusted and the crystals are controlled at the nanoscale, the diffusion performance of the molecular sieve can be effectively improved, its stability can be enhanced, and the specific selectivity for certain macromolecular products can also be improved.

[0009] The Chinese patent document with publication number CN116022820A discloses a method for preparing nanocrystalline Hβ molecular sieve by microwave heating. The patent crystallizes a mixture containing a silicon source, a template, water, an aluminum source and an optional non-polar base, controls the crystallization temperature within the range of 90 to 135°C by microwave radiation, and the crystallization time is less than or equal to 24 hours. 2The amount of silicon source, the amount of template agent is less than 0.2 mol, the amount of water is less than or equal to 10 mol, and the final synthesized nanocrystal particle size is less than or equal to 50 nm. Compared with conventional hydrothermal synthesis, this patent has the characteristics of low crystallization temperature, short crystallization time, and low water content in the system, but it still needs to add organic template agents with complex structure, high price and unfriendly environment, and it also needs to use unconventional microwave synthesis method, which limits its industrial application potential.

[0010] A Chinese patent document with publication number CN101723394B discloses a method for preparing a low silicon-aluminum ratio nano Hβ molecular sieve. The patent uses a low-cost FAU-configured microporous molecular sieve as an aluminum source to synthesize a nano Hβ molecular sieve under the conditions of adding a conventional silicon source and a non-toxic and inexpensive template. Although the cost of the raw material FAU molecular sieve used in the patent is low, it still needs to add an expensive and environmentally unfriendly organic template, which limits its industrial application potential. At the same time, the grain size of the prepared nano Hβ molecular sieve is above 100nm, and the grain size cannot be further reduced.

[0011] The above-mentioned methods for synthesizing nanocrystalline Hβ molecular sieves are all "bottom-up" strategies, that is, nanocrystalline Hβ molecular sieves are directly obtained by controlling the synthesis conditions. However, this method has complex processes and harsh reaction conditions, and usually requires the use of complex and expensive organic structure directing agents. In addition, the product yield is low, and the resulting product has a large grain size, which is not conducive to large-scale industrial production. Summary of the invention

[0012] The purpose of the present invention is to provide a method for preparing nanocrystalline Hβ molecular sieve by etching with ammonium fluoride in view of the shortcomings of the current technology. The method etches the commercial Hβ molecular sieve with an ammonium fluoride aqueous solution, and simultaneously performs desiliconization and dealumination, and while etching the internal defects between the crystals, the nanocrystalline Hβ molecular sieve is stripped and produced, and the nanocrystalline Hβ molecular sieve with a particle size of 20nm is successfully prepared by controlling the concentration, etching temperature and etching time of the ammonium fluoride aqueous solution; during the experiment, the ice-water mixture is used to perform suction filtration at a relatively low temperature and with a large amount of water dilution, thereby avoiding the secondary etching of ammonium fluoride during the suction filtration process.

[0013] The technical solution of the present invention is:

[0014] A method for preparing nanocrystalline Hβ molecular sieve by ammonium fluoride etching, the method comprising the following steps:

[0015] 1) Dry the Hβ molecular sieve at 100-130°C for 4-8 hours;

[0016] 2) adding the dried molecular sieve into an ammonium fluoride solution and chemically etching for 5 min to 120 min at 20° C. to 50° C., with mechanical stirring and ultrasonic waves;

[0017] Wherein, 5 to 15 g of Hβ molecular sieve is added to every 200 g of aqueous solution of ammonium fluoride, and the concentration of the ammonium fluoride solution is 20 wt% to 40 wt%;

[0018] 3) At a temperature of 0 to 4° C., the etched solution obtained in the previous step is filtered by suction, and then the filter cake is washed with water; after washing until the pH of the filtrate is above 6.5, the filter cake is dried to obtain a nanocrystalline Hβ molecular sieve;

[0019] Preferably, in step 3), the concentration of the ammonium fluoride aqueous solution is 40 wt %; the etching temperature is 50° C.; and the etching time is 15 min.

[0020] The nanocrystalline Hβ molecular sieve prepared by the method is used for preparing a supported metal-acid dual-functional catalyst.

[0021] The method specifically comprises the following steps: adopting a conventional equal volume impregnation method to prepare a supported metal-acid bifunctional catalyst, wherein the supported amount is 0.5% to 1%; and the catalyst particle size is 40-60 meshes.

[0022] The metal is one or both of Pt and Pd;

[0023] The supported metal-acid bifunctional catalyst is used for isomerization of n-hexadecane.

[0024] n-Hexadecane and hydrogen are introduced into a fixed bed reactor at 240-320°C, 2-3 MPa, and a space velocity of 6-32 h -1 , obtaining a mixture of hexadecane isomers and cracking products;

[0025] Wherein, the volume ratio of hydrogen to n-hexadecane is 500-1500:1;

[0026] Preferably, the hydrogen flow rate is 66.5 mL / min, and the n-hexadecane flow rate is 0.08 mL / min;

[0027] The essential features of the present invention are:

[0028] The current technologies for synthesizing nanocrystalline Hβ molecular sieves all adopt a "bottom-up" strategy, that is, synthesizing nanocrystalline Hβ molecular sieves in situ by controlling conditions.

[0029] Since the Hβ molecular sieve has a nanocrystal symbiotic polycrystalline structure, the internal interfaces between the crystals can lead to mismatches in structure and pore arrangement, thereby affecting the internal diffusion barrier of the Hβ molecular sieve. Research shows that the nanocrystal region is a highly crystalline region, and the internal interface is a highly defective region. Based on this, the present invention proposes a "top-down" strategy, that is, by means of post-treatment with ammonium fluoride etching, nanocrystalline Hβ molecular sieve is exfoliated from commercial Hβ molecular sieve. This method can selectively etch the defective structure in the Hβ molecular sieve without damaging the highly crystalline region in the molecular sieve. By simultaneously etching the Si and Al elements of the defective structure, intercrystalline mesopores of the nanocrystals are formed, and the Hβ molecular sieve nanocrystals are exfoliated.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] 1) Adopt a "top-down" strategy, that is, use industrial commercial Hβ molecular sieve to synthesize nanocrystalline Hβ molecular sieve by post-treatment with ammonium fluoride etching. Relative to the Hβ molecular sieve matrix, as the etching degree deepens (Hβ-P < Hβ-6 < Hβ-7 < Hβ-9 < Hβ-2 < Hβ-1), the hysteresis loop gradually increases, indicating that the mesoporous structure in the sample gradually increases with the deepening of the etching degree. From Figure 2 The BJH pore size distribution curve of typical samples shows that as the etching degree deepens, the large mesopores with a pore size of more than 5 nm gradually increase, and the most probable pore size of the mesopores gradually increases from 8 nm to 16 nm. Through ammonium fluoride etching treatment, mesopores can be effectively introduced into the Hβ molecular sieve, and with the deepening of the etching degree, more introduced mesoporous pores are formed.

[0032] 2) Compared with the traditional "bottom-up" strategy for in-situ synthesis of nanocrystalline Hβ molecular sieve, the present invention does not use organic templating agents with complex structures, high prices and environmental unfriendliness, and at the same time has the advantages of simple process and controllable conditions.

[0033] 3) Compared with the prior art, the present invention successfully prepares nanocrystalline Hβ molecular sieve with a grain size of 20 nm. From Figure 5 The TEM images of two molecular sieve samples, the comparative sample Hβ-P and the sample Hβ-1 of Example 1, show that the parent Hβ-P sample exists in the form of a polycrystalline aggregate composed of nanocrystal symbiosis with a large number of internal interfaces. After being treated under the most severe ammonium fluoride etching conditions, there are nanocrystals of about 20 nm and obvious intercrystalline mesopores in the Hβ-1 sample.

[0034] 4) The nanocrystalline Hβ molecular sieve after ammonium fluoride etching shows excellent isomerization performance in the isomerization reaction of long-chain alkanes. From Figure 7The yields of different products show that the yield of isomeric products exhibited by the Pt / Hβ-1 catalyst prepared by post-treatment with ammonium fluoride etching is better than that of the Pt / Hβ-P catalyst without post-treatment with ammonium fluoride. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is the N of different Hβ samples obtained in Examples 1, 2, 6, 7, and 9 2 Physical adsorption-desorption isotherms.

[0036] Figure 2 : BJH pore size distribution curves of different Hβ samples obtained in Examples 1, 2, 6, 7, and 9.

[0037] Figure 3 These are SEM images of different Hβ samples obtained in Examples 1, 2, 6, 7, and 9.

[0038] Figure 4 This is a high-magnification SEM image of the Hβ-1 sample obtained in Example 1.

[0039] Figure 5 TEM images of Hβ-P and Hβ-1 samples obtained in Example 10 and 1; wherein, Figure 5 a is the TEM image of Hβ-P sample; Figure 5 b is the TEM image of Hβ-1 sample.

[0040] Figure 6 is a graph showing the change of the reactant conversion rate with the reaction temperature for the isomerization reaction of n-hexadecane catalyzed by the Pt / Hβ-P and Pt / Hβ-1 samples obtained in Example 10 and 1;

[0041] Figure 7 The product yield diagram of the isomerization reaction of n-hexadecane catalyzed by the Pt / Hβ-P and Pt / Hβ-1 samples obtained in Example 10 and 1; wherein, Figure 7 a is the product yield diagram of Pt / Hβ-P sample; Figure 7 b is the product yield diagram of Pt / Hβ-1 sample; DETAILED DESCRIPTION

[0042] The Hβ molecular sieve involved in the present invention is a commercially available known material, specifically the NKF-6 (β) powdered molecular sieve produced by Tianjin Nanhua Catalyst Co., Ltd., with a relative crystallinity of ≥95%; but not limited thereto.

[0043] Example 1

[0044] 1) Place about 10 g of Hβ molecular sieve in an oven at 120°C and dry for 6 hours.

[0045] 2) The dried molecular sieve was added into 200 g of a 40 wt % aqueous solution of ammonium fluoride, and chemically etched for 15 min under mechanical stirring and ultrasonic action at 50° C. The product was named Hβ-1.

[0046] Prepare ice water and a large Buchner funnel in advance. Dilute the sample with a large amount of water at 0°C and filter until the pH of the filtrate is above 6.5.

[0047] 3) The filtered sample was placed in an oven at 110°C and dried for 8 h.

[0048] 4) Weigh 5 g of dried Hβ-1 molecular sieve sample and calculate the amount of chloroplatinic acid (H 2 PtCl 6 6H 2 O) The volume of the standard solution (concentration 1%) is 2.5 mL.

[0049] Use a pipette to add the chloroplatinic acid standard solution to the crucible containing the Hβ-1 molecular sieve catalyst sample, and add deionized water drop by drop while stirring until the sample reaches the saturated water absorption (the sum of the added amount of chloroplatinic acid standard solution and the added amount of deionized water is equal to the saturated water absorption of the catalyst, and the substance in the crucible is in the form of "toothpaste").

[0050] 5) The samples with equal volumes of impregnation were first air-dried at room temperature for 24 hours and then dried in an oven at 120°C for 12 hours.

[0051] 6) The dried sample was placed in a muffle furnace, heated to 450°C at a rate of 2°C / min, and calcined for 4 hours. The obtained sample was named Pt / Hβ-1.

[0052] Embodiment 2-9

[0053] All steps of this embodiment are consistent with those of embodiment 1, except that the concentration of the ammonium fluoride aqueous solution, the etching temperature and the etching time are different, as follows, wherein Hβ-P is a molecular sieve comparison sample that has not been etched with ammonium fluoride but only dried.

[0054] Table 1

[0055]

[0056] The Hβ molecular sieve used in Examples 1-9 is a nanocrystalline co-growth polycrystalline structure. The internal interface between the crystals will cause a mismatch in structure and pore arrangement, thereby affecting the internal diffusion barrier of the Hβ molecular sieve. The nanocrystalline region is a highly crystalline region, and the internal interface is a highly defective region. The ammonium fluoride post-treatment method used in Examples 1-9 can selectively etch the defect structure in the Hβ molecular sieve without destroying the highly crystalline region in the molecular sieve. By simultaneously etching the Si and Al elements of the defect structure, intercrystalline mesopores of the nanocrystals are formed, and the Hβ molecular sieve nanocrystals are peeled off.

[0057] The specific surface area, pore structure and other data of Examples 1-9 and the comparison sample Hβ-P were characterized using the ASAP-2020 nitrogen physical adsorption instrument from Micromeritics, USA. Before the test, about 100 mg of the sample was weighed and degassed at 250°C for 12 hours under vacuum conditions. After the pretreatment, the sample was placed in liquid nitrogen (77K) for testing. The adsorption isotherm type of the sample can be used to analyze the pore structure of the sample. The BET method is used to analyze the total specific surface area of ​​the sample, the t-plot method is used to analyze the micropore specific surface area and micropore volume of the sample, and the HK method is used to analyze the micropore pore size distribution curve of the sample. The relevant data are summarized in Table 2.

[0058] Table 2

[0059]

[0060] Combining Table 1 and Table 2, it can be seen that when the ammonium fluoride concentration and etching temperature are the same, as the etching time increases, the external specific surface area S External and the mesopore volume V mesopore gradually increases, while the micropore specific surface area S micropore and micropore volume V micropore Gradually decreases; under the same etching temperature and time conditions, with the increase of ammonium fluoride concentration, the external specific surface area and mesopore volume of the sample gradually increase, while the micropore specific surface area and micropore volume gradually decrease; with the increase of etching temperature, the external specific surface area and mesopore volume of the sample gradually increase, while the micropore specific surface area and micropore volume gradually decrease; the parent Hβ-P sample has the most micropores and the least mesopores. The micropore volume of the Hβ-1 sample with the most stringent etching conditions and the deepest etching degree decreases by 41%, while the mesopore volume increases by 454%.

[0061] Depend on Figure 1 It can be seen that the N of typical samples (comparative sample Hβ-P and examples 1, 2, 6, 7, 9) 2Both the physical adsorption and desorption curves exhibit type-IV adsorption isotherms, with significant changes in the adsorption amount at both low and high pressures, indicating the coexistence of micropores and mesopores. Compared with the parent Hβ zeolite, as the etching degree increases (Hβ-P < Hβ-6 < Hβ-7 < Hβ-9 < Hβ-2 < Hβ-1), the hysteresis loop gradually enlarges, suggesting that the mesoporous structure in the samples gradually increases with the deepening of the etching degree.

[0062] From Figure 2 The BJH pore size distribution curves of typical samples show that with the increase of the etching degree, the large mesopores with a pore size above 5 nm gradually increase, and the most probable pore size of the mesopores gradually increases from 8 nm to 16 nm. In summary, the ammonium fluoride etching treatment can effectively introduce mesopores into Hβ zeolite, and with the deepening of the etching degree, more mesoporous pores are introduced.

[0063] The scanning electron microscope (SEM) was used to observe the crystal microtopography of the synthesized samples. The instrument used was the Regulus 8100 scanning electron microscope of Hitachi. The secondary electron resolution of the instrument is 0.8 nm at 15 kV and 1.1 nm at 1 kV, and the acceleration voltage is 0.1 - 30 kV. When preparing the sample, the sample was first ground into a fine powder, then smeared on the conductive adhesive attached to the sample stage with a toothpick, and platinum was sputtered for 80 s at a voltage of 10 kV in a sputtering coater.

[0064] From Figure 3 The SEM images of typical samples (control sample Hβ-P and Examples 1, 2, 6, 7, 9) show that the parent Hβ zeolite is composed of a large number of small crystals closely packed and symbiotically forming an irregular polycrystalline aggregate of 100 - 400 nm, with a relatively rough surface and an unclear external shape; the zeolite samples treated with ammonium fluoride still maintain a morphology similar to that of the parent sample Hβ-P, but the surface roughness is significantly improved; with the increase of the etching degree, the change in the surface morphology of the sample increases, the gaps between the originally closely packed small crystals increase, and a small amount of particles are peeled off from the polycrystalline aggregate, showing a gradually separated trend between the particles;

[0065] From Figure 4 The SEM image of sample Hβ-1 of Example 1 at a higher magnification (100k) shows that the ammonium fluoride etching treatment introduces a large number of intercrystalline mesopores of 10 - 20 nm in the polycrystals and exfoliates nanocrystals of about 20 nm from the polycrystals.

[0066] The TEM images of the samples were observed using the JEM-F200 equipment of JEOL, Japan, and the acceleration voltage of the electron beam was 200 kV. From Figure 5From the TEM images of the two molecular sieve samples, the comparative sample Hβ-P and Example 1 Hβ-1, it can be seen that the parent Hβ-P sample exists in the form of a polycrystalline aggregate composed of intergrowth of nanocrystals with a large number of internal interfaces. After being treated under the most stringent ammonium fluoride etching conditions, the Hβ-1 sample has nanocrystals of about 20nm and obvious intercrystalline mesopores. The results of the TEM image and the SEM image are highly consistent, both indicating that the parent Hβ-P sample is a polycrystalline aggregate composed of intergrowth of nanocrystals, while the Hβ-1 sample is a 20nm nanocrystal with highly exposed surface and obvious intercrystalline mesopores.

[0067] Example 10

[0068] 1) The unetched commercial Hβ molecular sieve was placed in an oven at 110°C and dried for 8 h.

[0069] 2) Weigh 5 g of dried Hβ molecular sieve sample and calculate the amount of chloroplatinic acid (H 2 PtCl 6 6H 2 O) The volume of the standard solution (concentration 1%) is 2.5 mL.

[0070] 3) Use a pipette to add the chloroplatinic acid standard solution to the crucible containing the Hβ molecular sieve catalyst sample, and add deionized water drop by drop, stirring while adding, until the saturated water absorption of the sample is reached (the sum of the amount of chloroplatinic acid standard solution added and the amount of deionized water added is equal to the saturated water absorption of the catalyst, and the substance in the crucible is in the form of "toothpaste").

[0071] 4) The samples with equal volumes of impregnation were first air-dried at room temperature for 24 hours and then placed in an oven at 120°C for 12 hours.

[0072] 5) The dried sample was placed in a muffle furnace, heated to 450°C at a rate of 2°C / min, and calcined for 4 h. The obtained sample was named Pt / Hβ-P.

[0073] The Pt / Hβ catalyst synthesized in this example was used for the isomerization reaction of n-hexadecane. A fixed bed reactor was used, the inner diameter of the reaction tube was 10 mm, the flow rate of n-hexadecane was 0.08 mL / min, the amount of catalyst added was 0.1125 g, and the space velocity was 32 h -1 , the catalyst particle size is 40-60 mesh, the reaction pressure is 2MPa, the hydrogen flow rate is 66.5mL / min, and the reaction conversion rate is changed by adjusting the reaction temperature between 240 and 300°C. The gas components enter the online chromatogram through the tail back pressure valve for analysis, and the liquid components are collected and analyzed using the offline chromatogram. Both the online and offline chromatograms use FID detectors to detect and analyze the products.

[0074] Depend on Figure 6 The curve of the change of reactant conversion rate with reaction temperature shows that: whether it is Pt / Hβ-P or Pt / Hβ-1, the reactant conversion rate increases with the increase of reaction temperature and finally tends to be constant. The reactant conversion rate can be effectively adjusted by adjusting the reaction temperature. According to the type of reaction products, the products of the n-hexadecane isomerization reaction can be divided into single-branched isomers, multi-branched isomers, and cracking products. Since the n-hexadecane isomerization reaction is a continuous reaction, the product distribution changes with the change of conversion rate. Therefore, it is necessary to compare the product distribution under different conversion rates to analyze the difference between the two catalysts.

[0075] Depend on Figure 7 From the yields of various products under different conversion rates, it can be seen that: with the deepening of the etching degree, the yield of single-branched isomers increased from 22.7% of Pt / Hβ-P catalyst to 24.2% of Pt / Hβ-1 catalyst, and the yield of multi-branched isomers increased from 38.5% of Pt / Hβ-P catalyst to 45.2% of Pt / Hβ-1 catalyst. The yield of isomerized products shown by Pt / Hβ-1 catalyst prepared by ammonium fluoride etching post-treatment is better than the yield of isomerized products shown by Pt / Hβ-P catalyst without ammonium fluoride post-treatment.

[0076] It can be seen from the above examples that compared with the existing methods, the present invention does not need to use complex and expensive organic templates, and has the advantages of simple process and environmental friendliness. By optimizing the etching conditions, the Hβ molecular sieve nanocrystals were finally reduced to a scale of 20nm for the first time. By isovolumetric impregnation of metal Pt, metal-acid bifunctional Pt / Hβ catalysts of different grain sizes were prepared and applied to the isomerization reaction of long-chain alkanes. The Pt / Hβ catalyst prepared by ammonium fluoride etching and process optimization showed better isomer yield than the untreated Pt / Hβ catalyst.

[0077] Matters not covered by the present invention are known technologies.

Claims

1. A method for preparing nanocrystalline Hβ molecular sieve by ammonium fluoride etching, characterized in that the method comprises the following steps: 1) Dry the Hβ molecular sieve at 100-130°C for 4-8 hours; 2) adding the dried molecular sieve into an ammonium fluoride solution and chemically etching for 5 min to 120 min at 20° C. to 50° C., with mechanical stirring and ultrasonic waves; Wherein, 5-15 g Hβ molecular sieve is added to every 200 g of ammonium fluoride aqueous solution, and the concentration of the ammonium fluoride solution is 20 wt% to 40 wt%; 3) At a temperature of 0 to 4° C., the etched solution obtained in the previous step is filtered, and then the filter cake is washed with water; after washing until the pH of the filtrate is above 6.5, the filter cake is dried to obtain a nanocrystalline Hβ molecular sieve.

2. The method for preparing nanocrystalline Hβ molecular sieve by ammonium fluoride etching according to claim 1, characterized in that In step 3), the concentration of the ammonium fluoride aqueous solution is 40 wt %; the etching temperature is 50° C.; and the etching time is 15 min.

3. The use of the nanocrystalline Hβ molecular sieve prepared by the method according to claim 1, characterized in that it is used for Preparation of supported metal-acid bifunctional catalysts.

4. The use according to claim 3, characterized in that The supported metal-acid bifunctional catalyst is prepared by conventional equal volume impregnation method, the loading amount is 0.5% to 1%; the catalyst particle size is 40-60 mesh; The metal is one or both of Pt and Pd.

5. The use according to claim 4, characterized in that the supported metal-acid bifunctional catalyst is used for isomerization of n-hexadecane; The method comprises the following steps: introducing n-hexadecane and hydrogen into a fixed bed reactor at 240-320°C, 2-3 MPa, and a space velocity of 6-32 h -1 , obtaining a mixture of hexadecane isomers and cracking products; in, The volume ratio of hydrogen to n-hexadecane is 500-1500:

1.

6. The use as claimed in claim 5, characterized in that the hydrogen flow rate is 66.5 mL / min and the n-hexadecane flow rate is 0.08 mL / min.

Citation Information

Patent Citations

  • Method for producing high-purity electronic grade ammonium fluoride etching solution with liquid phase method

    CN102627298A