Composite flocculant and treatment method of shield waste soil slurry
By using composite flocculants in the treatment of shield waste soil slurry, including modified mafen flocculants, modified chitosan, polyacrylamide and modified activated carbon, the flocculation effect and slow speed are solved, and high efficiency is achieved. Economical mud treatment achieves the purification effect of pollutants and heavy metals.
Patent Information
- Application Number
- CN202411448258.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-10-17
AI Technical Summary
The existing flocculants have problems such as poor flocculation effect and slow flocculation speed in the treatment of shield waste soil slurry, resulting in low processing efficiency and high cost.
Compound flocculants, including modified maflox flocculants, modified chitosan, polyacrylamide and modified activated carbon, are used to add them to the mud at different times, and the flocculation effect and efficiency are enhanced by inorganic and organic composite.
It improves the flocculation effect and speed of flocculant, reduces the treatment cost, effectively reduces the zeta potential of colloidal particles, enhances adsorption and settlement capabilities, improves the treatment effect and efficiency of wastewater and waste mud, and meets the emission standards.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flocculants, and in particular to a composite flocculant and a method for treating shield waste soil slurry. Background Art
[0002] Shield tunnel construction has the advantages of high excavation efficiency and little impact on the surrounding environment, so it is widely used in subway construction projects. Mud, as an engineering auxiliary material, is widely used in bored pile construction, shield excavation construction and underground continuous wall construction. Mud mainly plays the role of wall protection, slag removal, hole cleaning and cooling. When the mud has performance deterioration problems such as increased viscosity and fine particles, the mud will be discarded. Due to the large output, high viscosity and difficulty in solid-liquid separation of waste mud, the disposal of waste mud has become a major problem in engineering construction. The generation of a large amount of waste mud will not only cause a waste of land area, but also may cause pollution to the soil of the landfill. Therefore, the reduction of waste mud is a key step in resource treatment. The current common treatment methods include external landfill, mechanical filtration, curing agent curing treatment and flocculant precipitation dehydration. What's more, the waste mud is directly discharged into rivers, which not only causes serious pollution, but also causes siltation of water areas and elevation of riverbeds. External landfill is a high-cost but low-efficiency treatment method; although mechanical filter pressing has improved efficiency, the equipment operating cost is high and requires regular maintenance; solidification treatment with solidifying agents requires that the treated soil has a certain carrying capacity, otherwise it cannot be reused; flocculation sedimentation can use flocculants to form larger flocs of suspended particles in the mud, and auxiliary mechanical means to make the solid and liquid phases easier to separate, which can reduce the discharge of waste mud from the source. It is a dehydration method that can be widely used in actual engineering.
[0003] However, most of the flocculants on the market currently have problems such as poor flocculation effect or slow flocculation speed, high cost, etc. For example, the Chinese patent (CN109354141A) discloses a flocculant formula for shield waste slurry treatment, including the following components: PAC with a purity of 30% and PAM with a molecular weight of 12 million. When the waste slurry has a specific gravity of 1.05g / cm 3 When the dosage of PAC is 300mg / L, the dosage of PAM is 45mg / L. Although the patent formula selects suitable flocculants and dosages according to the different specific gravities of the mud, so that the mud can be flocculated and concentrated, its flocculation effect is limited and the flocculation speed is slow. Therefore, how to prepare a flocculant with good flocculation effect, fast flocculation speed, economy and environmental protection for shield mud treatment is an urgent problem to be solved. Summary of the invention
[0004] The main purpose of the invention is to provide a composite flocculant and a method for treating shield waste soil slurry, aiming to solve the problems of poor flocculation effect and slow flocculation speed of the existing flocculants.
[0005] To achieve the above object, the present invention provides a composite flocculant, comprising flocculant A and flocculant B, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan; and the flocculant B comprises polyacrylamide and modified activated carbon.
[0006] Preferably, the preparation method of the improved magnesium iron flocculant comprises the following steps: MgO and FeSO4·7H2O are mixed according to the number of magnesium-iron molecules (2-4): (6-8), and then concentrated sulfuric acid is added and stirred evenly to obtain a mixed solution; NaClO3 is dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution is added to the mixed solution at one time while stirring, and then reacted at 25-35°C for 0.5-1.5h, cooled, and a modified magnesium-iron flocculant is obtained.
[0007] Preferably, the preparation method of the modified chitosan comprises the following steps: Add isopropanol and acetic acid to chitosan, stir to dissolve, then slowly add epichlorohydrin, heat to react, and obtain an epoxidized chitosan product. Add hexadecyldimethylbenzylammonium chloride to the epoxidized chitosan product, react at 50-70°C for 5-6h to obtain modified chitosan.
[0008] Preferably, the usage ratio of chitosan, epichlorohydrin and hexadecyldimethylbenzyl ammonium chloride is (10-30 g): (20-50 mL): (1-2 g); The temperature of the heating reaction is 40-60° C., and the time of the heating reaction is 3-5 hours.
[0009] Preferably, the mass ratio of the flocculant A to the flocculant B is (0.5-5): (0.1-0.5); The mass ratio of the improved magnesium iron flocculant and the modified chitosan is (2-5): (1-3); The mass ratio of the polyacrylamide to the modified activated carbon is (3-6): (2-5).
[0010] Preferably, the preparation method of the modified activated carbon comprises the following steps: The waste straw is crushed and sieved, and then a sodium hydroxide solution is added, soaked for a period of time, and then carbonized at high temperature to obtain biochar, which is washed, dried, ground and sieved to obtain activated carbon; concentrated sulfuric acid is added to the activated carbon, and after stirring, potassium permanganate is slowly added and stirred continuously, after reacting for a period of time, washed and dried to obtain oxidized activated carbon; anhydrous ethanol is added to the oxidized activated carbon, and hydrochloric acid is added to adjust the pH value to 3-4, and after stirring evenly, (3-mercaptopropyl) triethoxysilane and hexadecyltrimethylammonium bromide are slowly added dropwise, and heated to react to obtain modified activated carbon.
[0011] Preferably, the concentration of the sodium hydroxide solution is 1-2 mol / L, the temperature of the high-temperature carbonization is 650-850°C, and the temperature of the heating reaction is 60-80°C.
[0012] Preferably, the mass ratio of the activated carbon to potassium permanganate is 1:(2-4); the dosage ratio of the oxidized activated carbon, (3-mercaptopropyl)triethoxysilane and hexadecyltrimethylammonium bromide is (6-10 g):(2-4 mL):(1-3 mL).
[0013] The present invention also provides a method for treating shield waste soil slurry. In the treatment project of shield waste soil slurry, the composite flocculant as described above is used.
[0014] Preferably, the method comprises the following steps: S1, collecting waste soil slurry, letting it stand for a period of time, and then filtering it to obtain sand particles and filtered slurry; S2, sending the filtered mud in step S1 into a sedimentation tank, adding a modified magnesium iron flocculant, stirring evenly, keeping warm and standing for 10-20 minutes, and then adding modified chitosan, stirring, and standing to obtain a preliminary treated mud; wherein the sum of the mass of the modified magnesium iron flocculant and the modified chitosan in the flocculant A accounts for 0.5% to 5% of the mud volume; S3, adding 0.1% to 0.5% of flocculant B to the preliminary treated mud, and stirring evenly; wherein the flocculant B includes polyacrylamide and modified activated carbon; S4, sending the mud into the filter press for dehydration and separation, and collecting the separated clear liquid and mud cake; S5. Use the sand particles in step S1 and the mud cake in step S4 as shield sand or for backfilling; and directly discharge the clear liquid in step 4.
[0015] Compared with the prior art, the beneficial effects of the present invention are: (1) The composite flocculant provided by the present invention is compounded with a modified magnesium iron flocculant, modified chitosan, polyacrylamide, and modified activated carbon, and is added to the shield mud at different times. The inorganic and organic composite method is adopted to make up for the many shortcomings of a single type of flocculant, give full play to the flocculation advantages of each type, and improve the treatment efficiency while reducing the treatment cost.
[0016] (2) The improved magnesium iron flocculant provided by the present invention has lower cost than traditional polyferric sulfate, and can be adsorbed by negatively charged colloids in the mud, reducing the absolute value of the zeta potential of the colloid surface, reducing the repulsive potential energy in the mud, reducing the stability of the colloid particles, and increasing the probability of collision between each other, and finally the colloid is destabilized and precipitated and separated from the water; the modified chitosan provided by the present invention is first epoxidized by chitosan, and then subjected to a substitution reaction to obtain a modified chitosan with a quaternary ammonium group and a benzyl group, so that the flocculant has strong surface activity and hydrophobic association effect, and at the same time, the quaternary ammonium group enhances the electrical neutralization ability of the flocculant, adsorbs the colloid particles on the surface of the flocculant, and neutralizes the negative charge on the surface of the colloid. The charge reduces the zeta potential value of the colloid surface, reduces the electrostatic repulsion, and further destabilizes the colloid. Finally, under the action of adsorption electrical neutralization, the colloid particles are condensed and aggregated and removed. The modified activated carbon provided by the present invention is prepared from waste straw, which has a wide source and saves resources. The waste straw is carbonized and then modified to introduce thiol groups, which, on the one hand, improves the adsorption bridging effect of the flocculant, and on the other hand, can enhance the ability to adsorb heavy metals such as copper, lead, chromium and the like in water, so that the treated water meets the discharge standard. At the same time, there is a hydrogen bond between the modified chitosan and the modified activated carbon, which enhances the effect of the flocculant in removing suspended particles during flocculation and sedimentation, thereby making the colloids in the water more efficiently removed.
[0017] (3) The improved magnesium iron flocculant, modified chitosan, polyacrylamide, and modified activated carbon provided by the present invention can greatly improve the effect and efficiency of wastewater and waste sludge treatment through the synergistic effects of flocculation-adsorption, charge neutralization, adsorption bridging, pore structure, and composite materials.
[0018] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments. DETAILED DESCRIPTION
[0019] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0020] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0021] Example 1
[0022] A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 10:1, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan in a mass ratio of 3:2; and the flocculant B comprises polyacrylamide and modified activated carbon in a mass ratio of 4:3; The preparation method of the improved magnesium-iron flocculant comprises the following steps: 12g MgO and 195g FeSO4·7H2O were mixed, and then 100mL concentrated sulfuric acid was added and stirred to obtain a mixed solution; 10g NaClO3 was dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution was added to the mixed solution at one time while stirring, and then reacted at 30°C for 1h, and cooled to obtain a modified magnesium-iron flocculant; The preparation method of the modified chitosan comprises the following steps: Add 30 mL of isopropanol and 20 mL of acetic acid to 20 g of chitosan, stir to dissolve, then slowly add 30 mL of epichlorohydrin, react at 50 ° C for 4 h to obtain an epoxidized chitosan product, add 1.5 g of hexadecyl dimethyl benzyl ammonium chloride to the epoxidized chitosan product, react at 60 ° C for 5.5 h to obtain a modified chitosan; The preparation method of the modified activated carbon comprises the following steps: 100g of waste straw was crushed and sieved, and then added with 1.5mol / L sodium hydroxide solution, soaked for a period of time, and then carbonized at 700℃ to obtain biochar, which was washed, dried, ground and sieved to obtain activated carbon; 200mL of concentrated sulfuric acid was added to 10g of activated carbon, and after stirring, 30g of potassium permanganate was slowly added and stirred continuously. After reacting for a period of time, it was washed and dried to obtain oxidized activated carbon; anhydrous ethanol was added to 8g of oxidized activated carbon, and 1mol / L hydrochloric acid was added to adjust the pH value to 3.5. After stirring evenly, 3mL of (3-mercaptopropyl)triethoxysilane and 2mL of hexadecyltrimethylammonium bromide were slowly added dropwise, and the mixture was heated to 70℃ for reaction for 5h to obtain modified activated carbon.
[0023] Example 2
[0024] A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 5:1, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan in a mass ratio of 2:1; and the flocculant B comprises polyacrylamide and modified activated carbon in a mass ratio of 3:2; The preparation method of the improved magnesium-iron flocculant comprises the following steps: 8 g of MgO and 167 g of FeSO4·7H2O were mixed, and then 90 mL of concentrated sulfuric acid was added and stirred to obtain a mixed solution; 10 g of NaClO3 was dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution was added to the mixed solution at one time while stirring, and then reacted at 30° C. for 1 hour, and cooled to obtain an improved magnesium-iron flocculant; The preparation method of the modified chitosan comprises the following steps: Add 20 mL of isopropanol and 20 mL of acetic acid to 10 g of chitosan, stir to dissolve, then slowly add 20 mL of epichlorohydrin, react at 40°C for 6 h to obtain an epoxidized chitosan product, add 1 g of hexadecyldimethylbenzylammonium chloride to the epoxidized chitosan product, react at 50°C for 6 h to obtain a modified chitosan; The preparation method of the modified activated carbon comprises the following steps: 80g of waste straw was crushed and sieved, and then 1mol / L sodium hydroxide solution was added and soaked for a period of time, followed by high-temperature carbonization at 650°C to obtain biochar, which was washed, dried, ground and sieved to obtain activated carbon; 180mL of concentrated sulfuric acid was added to 6g of activated carbon, and after stirring, 12g of potassium permanganate was slowly added and stirred continuously. After reacting for a period of time, the mixture was washed and dried to obtain oxidized activated carbon; anhydrous ethanol was added to 6g of oxidized activated carbon, and 1mol / L hydrochloric acid was added to adjust the pH value to 3. After stirring evenly, 2mL of (3-mercaptopropyl)triethoxysilane and 1mL of hexadecyltrimethylammonium bromide were slowly added dropwise, and the mixture was heated to 70°C for reaction for 5h to obtain modified activated carbon.
[0025] Example 3
[0026] A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 50:1, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan in a mass ratio of 5:3; and the flocculant B comprises polyacrylamide and modified activated carbon in a mass ratio of 6:5; The preparation method of the improved magnesium-iron flocculant comprises the following steps: 16g MgO and 220g FeSO4·7H2O were mixed, and then 110mL concentrated sulfuric acid was added and stirred to obtain a mixed solution; 10g NaClO3 was dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution was added to the mixed solution at one time while stirring, and then reacted at 30°C for 1h, and cooled to obtain an improved magnesium-iron flocculant; The preparation method of the modified chitosan comprises the following steps: Add 30 mL of isopropanol and 20 mL of acetic acid to 30 g of chitosan, stir to dissolve, then slowly add 50 mL of epichlorohydrin, react at 60 ° C for 3 h to obtain an epoxidized chitosan product, add 2 g of hexadecyldimethylbenzylammonium chloride to the epoxidized chitosan product, react at 70 ° C for 5 h to obtain a modified chitosan; The preparation method of the modified activated carbon comprises the following steps: 100g of waste straw was crushed and sieved, and then a 2mol / L sodium hydroxide solution was added and soaked for a period of time, followed by high-temperature carbonization at 850°C to obtain biochar, which was washed, dried, ground and sieved to obtain activated carbon; 200mL of concentrated sulfuric acid was added to 10g of activated carbon, and after stirring, 40g of potassium permanganate was slowly added and stirred continuously. After reacting for a period of time, the mixture was washed and dried to obtain oxidized activated carbon; anhydrous ethanol was added to 10g of oxidized activated carbon, and 1mol / L hydrochloric acid was added to adjust the pH value to 4. After stirring evenly, 4mL of (3-mercaptopropyl)triethoxysilane and 3mL of hexadecyltrimethylammonium bromide were slowly added dropwise, and the mixture was heated to 70°C for reaction for 5h to obtain modified activated carbon.
[0027] Comparative Example 1 A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 10:1, wherein the flocculant A comprises modified chitosan; and the flocculant B comprises polyacrylamide and modified activated carbon in a mass ratio of 4:3; Wherein, the preparation method of the modified chitosan comprises the following steps: Add 30 mL of isopropanol and 20 mL of acetic acid to 20 g of chitosan, stir to dissolve, then slowly add 30 mL of epichlorohydrin, react at 50 ° C for 4 h to obtain an epoxidized chitosan product, add 1.5 g of hexadecyl dimethyl benzyl ammonium chloride to the epoxidized chitosan product, react at 60 ° C for 5.5 h to obtain a modified chitosan; The preparation method of the modified activated carbon comprises the following steps: 100g of waste straw was crushed and sieved, and then added with 1.5mol / L sodium hydroxide solution, soaked for a period of time, and then carbonized at 700℃ to obtain biochar, which was washed, dried, ground and sieved to obtain activated carbon; 200mL of concentrated sulfuric acid was added to 10g of activated carbon, and after stirring, 30g of potassium permanganate was slowly added and stirred continuously. After reacting for a period of time, it was washed and dried to obtain oxidized activated carbon; anhydrous ethanol was added to 8g of oxidized activated carbon, and 1mol / L hydrochloric acid was added to adjust the pH value to 3.5. After stirring evenly, 3mL of (3-mercaptopropyl)triethoxysilane and 2mL of hexadecyltrimethylammonium bromide were slowly added dropwise, and the mixture was heated to 70℃ for reaction for 5h to obtain modified activated carbon.
[0028] Comparative Example 2 A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 10:1, wherein the flocculant A comprises a modified magnesium iron flocculant; and the flocculant B comprises polyacrylamide and modified activated carbon in a mass ratio of 4:3; The preparation method of the improved magnesium-iron flocculant comprises the following steps: 12g MgO and 195g FeSO4·7H2O were mixed, and then 100mL concentrated sulfuric acid was added and stirred to obtain a mixed solution; 10g NaClO3 was dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution was added to the mixed solution at one time while stirring, and then reacted at 30°C for 1h, and cooled to obtain a modified magnesium-iron flocculant; The preparation method of the modified activated carbon comprises the following steps: 100g of waste straw was crushed and sieved, and then added with 1.5mol / L sodium hydroxide solution, soaked for a period of time, and then carbonized at 700℃ to obtain biochar, which was washed, dried, ground and sieved to obtain activated carbon; 200mL of concentrated sulfuric acid was added to 10g of activated carbon, and after stirring, 30g of potassium permanganate was slowly added and stirred continuously. After reacting for a period of time, it was washed and dried to obtain oxidized activated carbon; anhydrous ethanol was added to 8g of oxidized activated carbon, and 1mol / L hydrochloric acid was added to adjust the pH value to 3.5. After stirring evenly, 3mL of (3-mercaptopropyl)triethoxysilane and 2mL of hexadecyltrimethylammonium bromide were slowly added dropwise, and the mixture was heated to 70℃ for reaction for 5h to obtain modified activated carbon.
[0029] Comparative Example 3 A composite flocculant, comprising flocculant A and flocculant B in a mass ratio of 10:1, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan in a mass ratio of 3:2; and the flocculant B comprises polyacrylamide; The preparation method of the improved magnesium-iron flocculant comprises the following steps: 12g MgO and 195g FeSO4·7H2O were mixed, and then 100mL concentrated sulfuric acid was added and stirred to obtain a mixed solution; 10g NaClO3 was dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution was added to the mixed solution at one time while stirring, and then reacted at 30°C for 1h, and cooled to obtain a modified magnesium-iron flocculant; The preparation method of the modified chitosan comprises the following steps: To 20 g of chitosan, add 30 mL of isopropanol and 20 mL of acetic acid, stir to dissolve, then slowly add 30 mL of epichlorohydrin, react at 50 ° C for 4 h to obtain an epoxidized chitosan product, add 1.5 g of hexadecyldimethylbenzylammonium chloride to the epoxidized chitosan product, react at 60 ° C for 5.5 h to obtain modified chitosan.
[0030] Test methods and results Shield slurry was collected, filtered, and divided into six parts. The composite flocculants in Examples 1 to 3 and Comparative Examples 1 to 3 were added in equal amounts to the six parts of slurry, wherein the improved ferrous magnesium flocculant in flocculant A was added first, stirred evenly, kept warm and allowed to stand for 15 minutes, and then modified chitosan was added, the sum of the masses of the ferrous magnesium flocculant and the modified chitosan accounted for 1% of the slurry amount, and then 0.3% of the slurry amount of flocculant B was added and stirred evenly; after standing for 1 hour, the slurry was sent to a filter press for dehydration and separation, the separated clear liquid and mud cake were collected, the clear liquid turbidity, total phosphorus, total nitrogen, COD value and mud cake moisture content were measured, and the turbidity removal rate was calculated.
[0031] Turbidity removal rate = [(shield sludge turbidity - filtrate turbidity) / shield sludge turbidity] * 100% Mud cake moisture content = [(mud cake weight obtained by filter pressing - mud cake weight after drying) / mud cake weight obtained by filter pressing] * 100%.
[0032] The representative pollutant content of shield mud is shown in Table 1 below.
[0033] Table 1 Representative pollutant content of shield mud
[0034] The clear liquids of Examples 1 to 3 and Comparative Examples 1 to 3 were respectively taken, and the residual concentrations of copper, lead and chromium, as well as the clear liquid turbidity, total phosphorus, total nitrogen, COD value and mud cake moisture content were determined by atomic absorption spectrophotometer, as shown in Table 2 below.
[0035] Table 2 Clear liquid turbidity, total phosphorus, total nitrogen, COD value and mud cake moisture content and clear liquid heavy metal content
[0036] It can be seen from Table 1 and Table 2 above that, compared with Comparative Examples 1 to 3, the flocculants prepared in Examples 1 to 3 of the present invention have better turbidity removal effects, and significantly reduce the water content of the mud cake, and have strong adsorption capacity for pollutants and heavy metals in the mud, achieving better purification effects, so that the purified water meets the discharge standards.
[0037] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A composite flocculant, characterized in that: It comprises flocculant A and flocculant B, wherein the flocculant A comprises a modified magnesium iron flocculant and modified chitosan; and the flocculant B comprises polyacrylamide and modified activated carbon; The preparation method of the improved magnesium iron flocculant comprises the following steps: MgO and FeSO4·7H2O are mixed according to the number of magnesium-iron molecules (2-4): (6-8), and then concentrated sulfuric acid is added and stirred evenly to obtain a mixed solution; NaClO3 is dissolved in deionized water to obtain a NaClO3 solution, and the NaClO3 solution is added to the mixed solution at one time while stirring, and then reacted at 25-35°C for 0.5-1.5h, cooled, and a modified magnesium-iron flocculant is obtained; The preparation method of the modified chitosan comprises the following steps: Add isopropanol and acetic acid to chitosan, stir and dissolve, then slowly add epichlorohydrin, heat and react to obtain an epoxidized chitosan product, add hexadecyldimethylbenzylammonium chloride to the epoxidized chitosan product, react at 50-70°C for 5-6h to obtain modified chitosan; The preparation method of the modified activated carbon comprises the following steps: The waste straw is crushed and sieved, and then a sodium hydroxide solution is added, soaked for a period of time, and then carbonized at high temperature to obtain biochar, which is washed, dried, ground and sieved to obtain activated carbon; concentrated sulfuric acid is added to the activated carbon, and after stirring, potassium permanganate is slowly added and stirred continuously, after reacting for a period of time, washed and dried to obtain oxidized activated carbon; anhydrous ethanol is added to the oxidized activated carbon, and hydrochloric acid is added to adjust the pH value to 3-4, and after stirring evenly, (3-mercaptopropyl) triethoxysilane and hexadecyltrimethylammonium bromide are slowly added dropwise, and heated to react to obtain modified activated carbon.
2. The composite flocculant according to claim 1, characterized in that The usage ratio of chitosan, epichlorohydrin and hexadecyl dimethyl benzyl ammonium chloride is (10-30 g): (20-50 mL): (1-2 g); The temperature of the heating reaction is 40-60° C., and the time of the heating reaction is 3-5 hours.
3. The composite flocculant according to claim 1, characterized in that The mass ratio of flocculant A to flocculant B is (0.5~5):(0.1~0.5); The mass ratio of the improved magnesium iron flocculant and the modified chitosan is (2-5): (1-3); The mass ratio of the polyacrylamide to the modified activated carbon is (3-6): (2-5).
4. The composite flocculant according to claim 1, characterized in that The concentration of the sodium hydroxide solution is 1-2 mol / L, the temperature of the high-temperature carbonization is 650-850°C, and the temperature of the heating reaction is 60-80°C.
5. The composite flocculant according to claim 1, characterized in that The mass ratio of the activated carbon to potassium permanganate is 1:(2-4); the dosage ratio of the oxidized activated carbon, (3-mercaptopropyl)triethoxysilane and hexadecyltrimethylammonium bromide is (6-10 g):(2-4 mL):(1-3 mL).
6. A method for treating shield waste soil slurry, characterized in that: In the treatment project of shield waste soil slurry, the composite flocculant as claimed in any one of claims 1 to 5 is used.
7. The method for treating shield waste soil slurry according to claim 6, characterized in that: The method comprises the following steps: S1, collecting waste soil slurry, letting it stand for a period of time, and then filtering it to obtain sand particles and filtered slurry; S2, sending the filtered mud in step S1 into a sedimentation tank, adding a modified magnesium iron flocculant, stirring evenly, keeping warm and standing for 10-20 minutes, and then adding modified chitosan, stirring, and standing to obtain a preliminary treated mud; wherein the sum of the mass of the modified magnesium iron flocculant and the modified chitosan in the flocculant A accounts for 0.5% to 5% of the mud volume; S3, adding 0.1% to 0.5% of flocculant B to the preliminary treated mud, and stirring evenly; wherein the flocculant B includes polyacrylamide and modified activated carbon; S4, sending the mud into the filter press for dehydration and separation, and collecting the separated clear liquid and mud cake; S5. Use the sand particles in step S1 and the mud cake in step S4 as shield sand or for backfilling; and directly discharge the clear liquid in step 4.
Citation Information
Patent Citations
Printing and dyeing wastewater coagulant as well as preparation method and application thereof
CN104556330A
Novel mud-water separation material for high-solid-content waste slurry and preparation method of novel mud-water separation material
CN107265826A
Ball-milling oxidation-sulfhydrylation modified biochar, and preparation method and application thereof
CN110639471A
Cationic starch-based flocculant as well as preparation method and application thereof
CN114920441A
Cited By
Separation, purification and characterization method for foreign matters in drinking water
CN121384554A
Directional crossing drilling waste slurry breaker and preparation method thereof
CN122853660A