Alkali-activated fly ash grouting material, preparation method and compaction pile construction method
Through alkali-activated fly ash grouting materials and tight pile construction methods, the problems of poor bearing capacity and stability of silt roadbed are solved, the tensile strength and crack resistance are improved, and the overall performance and road of silt roadbed are improved. Security.
Patent Information
- Application Number
- CN202411023169.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The silt roadbed is prone to deformation and liquefaction under vibrating loads, with poor bearing capacity and stability. The traditional reinforcement method is costly and has limited effect. The direct utilization of fly ash is not ideal.
The construction method of alkali-excited fly ash grouting materials and tight piles is adopted. The alkali-excited technology combines glass fiber, magnesium oxide fume and other materials to enhance the tensile strength, toughness and crack resistance of tight piles, and the tensile strength, toughness and crack resistance of tight piles are also used to extruded piles. Improve the bearing capacity and stability of silt roadbed.
It significantly improves the tensile strength and crack resistance of alkali-activated fly ash tight piles, enhances the bearing capacity and stability of the silt roadbed, realizes the resource utilization of industrial waste, and reduces environmental pollution and construction costs. .
Smart Images

Figure CN118955040A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road engineering, and in particular to an alkali-activated fly ash grouting material, a preparation method and a compaction pile construction method. Background Art
[0002] Silt is mainly formed by river transportation and deposition. The particle size distribution of silt is relatively simple, which makes it difficult to compact. It is prone to large deformation or even liquefaction under vibration load. It has poor bearing capacity and stability, which can easily cause road subsidence. To address this problem, traditional reinforcement methods such as direct compaction and replacement backfilling have problems such as high cost and limited effect. As an industrial waste, the resource utilization of fly ash has become a research hotspot. However, the effect of directly using fly ash to reinforce silt roadbed is not ideal.
[0003] A large number of studies have shown that alkali activation can improve the activity of fly ash and enhance its performance. For example, CN112250355A discloses an alkali-activated fly ash / slag recycled concrete, which makes full use of slag, fly ash industrial solid waste and construction waste, and improves the strength of recycled concrete through alkali activation. Fibers are also added to the raw materials to improve the flexural properties of recycled concrete and extend the service life of recycled concrete. However, the material ratio of the above scheme may have large porosity between materials, insufficient bonding between materials, large gaps in filling materials, insufficient density, and poor water stability, which can easily cause water damage to the roadbed. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an alkali-activated fly ash grouting material, a preparation method and a compaction pile construction method, which can enhance the tensile strength, toughness and crack resistance of alkali-activated fly ash compaction piles; improve the bearing capacity of silt roadbed by combining alkali activation technology with compaction piles; the construction process of compaction piles is simple, and can effectively improve the bearing capacity and stability of silt roadbed.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] In the first aspect, an embodiment of the present invention provides an alkali-activated fly ash grouting material, comprising the following raw materials in parts by weight: 480-550 parts of fly ash, 100-140 parts of alkali activator, 110-150 parts of steel slag, 100-130 parts of slag, 30-40 parts of glass fiber, 28-37 parts of magnesium oxide silica fume, 20-30 parts of silicone waterproofing agent, 15-22 parts of polyacrylamide, 15 parts of retarder, 10-15 parts of modified resin liquid, and a water-cement ratio of 0.39-0.41.
[0007] As a further implementation method, the combustion vector of fly ash is not greater than 10%, the content of SiO2+Al2O3+Fe2O3 is greater than 60%, the particle size is controlled at 0.05-3.0mm, the fineness of fly ash is not greater than 30%, and the fly ash content accounts for 50%-60% of the total mass of alkali-activated fly ash.
[0008] As a further implementation method, the amount of the alkali activator is 6%-10%, and other admixtures account for 15%-25% of the total mass.
[0009] As a further implementation, the dosage of the retarder is 1%-3%.
[0010] In a second aspect, an embodiment of the present invention further provides a method for preparing an alkali-activated fly ash grouting material, comprising the following steps:
[0011] The raw materials of the grouting material are mixed evenly, and then put into a mixer for stirring;
[0012] The uniformly stirred mixture is allowed to stand at room temperature for curing to allow the alkali-induced reaction to occur.
[0013] As a further implementation, the stirring speed of the stirrer is 500-600 rpm, and the stirring time is 30-40 minutes.
[0014] In a third aspect, an embodiment of the present invention further provides an alkali-activated fly ash compaction pile construction method, comprising the following steps:
[0015] The positions of compaction piles are arranged in an equilateral triangle;
[0016] The vibrating pile driver method is used for hole construction;
[0017] Filling the pile hole with filler, wherein the filler is layered and compacted on the pile top, and the filler is the alkali-activated fly ash grouting material;
[0018] After filling is completed, the compacted piles are maintained.
[0019] As a further implementation method, each pile hole is divided into 5-10 layers, and after each layer of filler is placed, a vibrating pile driver is used to vibrate and tamp the filler.
[0020] As a further implementation method, the first filling height is not less than 0.5m, and the number of vibration tamping is not less than 3 times;
[0021] Fill the pile hole with filler according to the principle that the next layer of filler should rise 0.5m-1m above the previous layer of filler.
[0022] As a further implementation method, the degree of compaction is controlled by measuring the compaction degree of the filler. The compaction standard is: measuring the compaction degree after a single vibration tamping, the compaction degree change of a single vibration tamping is no more than 2cm; or measuring the total compaction degree after three consecutive vibration tampings, the change is no more than 5cm.
[0023] The beneficial effects of the present invention are as follows:
[0024] (1) The present invention significantly enhances the tensile strength, toughness and crack resistance of alkali-activated fly ash compaction piles by incorporating glass fibers; the use of industrial waste materials such as fly ash and silica fume not only realizes the resource utilization of industrial waste and reduces costs, but also reduces environmental pollution; the bearing capacity of silt roadbed is improved by combining alkali-activated technology with compaction piles.
[0025] (2) The present invention enhances the bonding force between materials, fills the gaps between materials, and enhances the density by adding modified resin liquid.
[0026] (3) The compaction pile construction process of the present invention is simple and the construction speed is fast, which can effectively improve the bearing capacity and stability of the silt roadbed; by compacting the soil between the piles, the overall performance of the roadbed is further improved, ensuring the quality and safety of the road. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 It is a construction process diagram of the present invention;
[0029] Figure 2 is a pile hole position diagram in embodiment 4 of the present invention;
[0030] Figure 3 is a pile hole position diagram of embodiment 5 of the present invention;
[0031] Figure 4 It is a pile hole position diagram in Example 6 of the present invention. DETAILED DESCRIPTION
[0032] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0033] like Figure 1As shown, the present invention firstly uses fly ash, alkali activator, steel slag, slag, glass fiber, magnesium oxide silica fume, silicone waterproofing agent, polyacrylamide, retarder, and modified resin liquid to prepare green, environmentally friendly, and excellent performance grouting materials. Then, a vibrating pile driver is used to drive a steel pipe into the original silt of the roadbed to form a hole. After the hole is formed, the prepared grouting material is vibrated and compacted in layers to form a compacted pile, so that it is closely combined with the surrounding soil to form a composite foundation.
[0034] The invention provides an alkali-activated fly ash grouting material, which comprises the following raw materials in parts by weight: 480-550 parts of fly ash, 100-140 parts of alkali activator, 110-150 parts of steel slag, 100-130 parts of slag, 30-40 parts of glass fiber, 28-37 parts of magnesium oxide silica fume, 20-30 parts of organic silicon waterproofing agent, 15-22 parts of polyacrylamide, 15 parts of retarder, 10-15 parts of modified resin liquid, and the water-to-binder ratio is 0.39-0.41.
[0035] In some embodiments, the fly ash has a combustion vector of no more than 10%, SiO 2 +A l 2 O 3 +Fe 2 O 3 The content is greater than 60%, the particle size is controlled at 0.05-3.0mm, the fly ash fineness (45μm square hole sieve residue) is not more than 30%; the fly ash content accounts for 50% to 60% of the total mass of the alkali-activated fly ash.
[0036] The dosage of alkali activator is between 6% and 10%, and other admixtures account for 15% to 25% of the total mass. The specific proportion of each component can be adjusted according to specific engineering requirements to optimize the mechanical properties and durability of alkali-activated fly ash.
[0037] In some embodiments, sodium hydroxide (NaOH) and water glass (Na 2 SiO 3 ) as an alkali activator, wherein the concentration of sodium hydroxide is 10%-15% and the modulus of water glass is 2.0-3.0.
[0038] In some embodiments, the slag particle size does not exceed 10 mm and the specific surface area is not less than 400 m 2 / kg; the particle size of steel slag shall not exceed 15mm and the free calcium oxide content shall not exceed 4%.
[0039] In some embodiments, the magnesium oxide content in magnesium oxide silica fume is 5%, the average particle size of silica fume is between 0.1-0.3 μm, and the silicon dioxide content is not less than 88%; the active ingredient content of the organosilicon waterproofing agent is 15%, and the penetration depth reaches 6-12 mm.
[0040] The diameter of glass fiber monofilament is between 10-20 microns, and the tensile strength is not less than 320MPa. The molecular weight of polyacrylamide is between 5.5 million and 8 million, and the ionicity ranges between 10% and 40%.
[0041] The dosage of retarder is between 1% and 3%, which can be adjusted according to specific project requirements to control the setting time and working performance of alkali-activated fly ash.
[0042] In some embodiments, the retarder is mainly composed of borax (Na 2 B 4 O 7 10H 2 O); the solid content of the modified resin is 42%.
[0043] The preparation method of alkali activated fly ash grouting material is:
[0044] (1) mixing sodium hydroxide solution and water glass to prepare an alkali excitation solution;
[0045] (2) adding steel slag, slag and glass fiber into a mixer and mixing evenly;
[0046] (3) Add fly ash, magnesium oxide silica fume, silicone waterproofing agent, polyacrylamide, retarder, modified resin liquid and the alkali-activated solution of step (1) into the mixer of step (2), and continue to stir evenly to form an alkali-activated fly ash grouting material.
[0047] The uniformly stirred mixture is allowed to stand at room temperature for curing to allow the alkali-induced reaction to occur.
[0048] The present invention also provides an alkali-activated fly ash compaction pile construction method, comprising the following steps:
[0049] (1) Pile layout:
[0050] The arrangement of compaction piles is determined according to the geological conditions and design requirements of the silt roadbed. The distance between piles is generally 1.0-1.5m, arranged in an equilateral triangle.
[0051] (2) Hole forming construction:
[0052] The vibrating pile driver method is used for hole construction. The hole diameter is 50-70cm and the hole depth is 5-7m. The pile pipe should be kept vertical when driven in, with a deviation of no more than 2%. During the hole drilling process, attention should be paid to maintaining the stability of the hole wall to avoid hole collapse.
[0053] (3) Pile hole filling:
[0054] During the compaction pile construction process, the prepared alkali-activated fly ash grouting material is filled into the pile hole in batches and layers, and compacted layer by layer to meet the bearing capacity requirements.
[0055] In some embodiments, each pile hole is divided into 5-10 layers. After each layer of filler is placed in, a vibrating pile driver is used to vibrate and tamp the filler so that the soil layer within a certain range and depth at the bottom of the pile hole is compacted and reinforced; in this process, the height of the first filler is not less than 0.5m, and the number of vibration tamping is not less than 3 times.
[0056] The degree of compaction is then controlled by measuring the compaction degree of the filler, wherein the compaction degree standard is: measuring the compaction degree after a single vibration tamping, requiring that the compaction degree change of a single vibration tamping is not greater than 2cm; or measuring the total compaction degree after three consecutive vibration tampings, requiring that the change is not greater than 5cm.
[0057] The second layer construction area is 0.5m-1m higher than the first layer foundation, and the filler is continuously filled into the pile hole with a height of 0.5m-1m. The filled filler is vibrated and compacted using a vibrating pile driver. The filler is continuously vibrated and compacted on the second layer, so that the soil layer within a certain range and height around the pile hole is compacted and reinforced, and then the compaction degree is controlled by the same compaction degree standard as the first layer above; the third layer construction area is 0.5m-1m higher than the second layer foundation, and the filler is vibrated and compacted using the same method as the first and second layers above, and the compaction degree is controlled by the same compaction degree standard. Repeat the above operation to complete the filler vibrating and compacting operation of the fourth, fifth, sixth, etc. layers, and the compaction degree is controlled by the same compaction degree standard, and finally the construction of the compaction pile is completed, and it is ensured that the density of the pile body material and the soil around the pile from bottom to top is uniform and consistent, and the surrounding original silt roadbed is also better compacted and compacted laterally during the compaction pile compaction process.
[0058] After filling, the compaction piles are maintained to ensure that the alkali-activated fly ash slurry is fully hardened. The reinforced roadbed is quality tested, including bearing capacity test and settlement observation, to ensure that the reinforcement effect meets the design requirements.
[0059] The present invention utilizes the high performance of alkali-activated fly ash grouting materials to effectively improve the bearing capacity and stability of compaction piles, while achieving efficient utilization of fly ash, with significant environmental and economic benefits; it helps to improve the safety and durability of road projects, which is of great significance to improving the bearing capacity of roadbed under adverse geological conditions.
[0060] Embodiment 1:
[0061] An alkali-activated fly ash grouting material and a preparation method thereof, comprising the following steps:
[0062] Step 1: Pre-treat the materials and set them aside for later use.
[0063] Step 2: Weigh the raw materials by mass fraction, including 520 parts of fly ash, 115 parts of alkali activator, 115 parts of steel slag, 105 parts of slag, 32 parts of glass fiber, 32 parts of magnesium oxide silica fume, 26 parts of silicone waterproofing agent, 17 parts of polyacrylamide, 15 parts of retarder, and 12 parts of modified resin liquid.
[0064] Step 3: Put the above materials into a blender and mix evenly at a speed of 500-600 rpm for 30-40 minutes.
[0065] Step 4: Place the stirred material into a mold and cure it at room temperature for 28 days.
[0066] Embodiment 2:
[0067] An alkali-activated fly ash grouting material and a preparation method thereof, comprising the following steps:
[0068] Step 1: Pre-treat the materials and set them aside for later use.
[0069] Step 2: Weigh the raw materials by mass fraction, including 490 parts of fly ash, 105 parts of alkali activator, 120 parts of steel slag, 100 parts of slag, 30 parts of glass fiber, 28 parts of magnesium oxide silica fume, 22 parts of silicone waterproofing agent, 15 parts of polyacrylamide, 15 parts of retarder, and 10 parts of modified resin liquid.
[0070] Step 3: Put the above materials into a blender and mix evenly at a speed of 500-600 rpm for 30-40 minutes.
[0071] Step 4: Place the stirred material into a mold and cure it at room temperature for 28 days.
[0072] Embodiment 3:
[0073] An alkali-activated fly ash grouting material and a preparation method thereof, comprising the following steps:
[0074] Step 1: Pre-treat the materials and set them aside for later use.
[0075] Step 2: Weigh the raw materials by mass fraction, including 490 parts of fly ash, 105 parts of alkali activator, 155 parts of steel slag, 125 parts of slag, 35 parts of glass fiber, 22 parts of magnesium oxide silica fume, 22 parts of silicone waterproofing agent, 15 parts of polyacrylamide, 15 parts of retarder, and 10 parts of modified resin liquid.
[0076] Step 3: Put the above materials into a blender and mix evenly at a speed of 500-600 rpm for 30-40 minutes.
[0077] Step 4: Place the stirred material into a mold and cure it at room temperature for 28 days.
[0078] Comparative Example 1:
[0079] The difference between Comparative Example 1 and Example 1 is that the modified resin liquid in the raw material component of Example 1 is not added, and the other conditions are the same as Example 1. Comparative Example Comparative Example 1, Example 2, and Example 3, the alkali-activated fly ash filling material prepared by using the modified resin liquid and the alkali-activated fly ash filling material prepared without adding the modified resin liquid are subjected to performance tests, and the test results are shown in Table 1:
[0080] Table 1
[0081] Compressive strength / MPa Coagulation time / min Water absorption / % Example 1 45.2 38 3.2 Example 2 46.3 46 4.1 Example 3 45.7 51 3.8 Comparative Example 1 41.8 40 5.2
[0082] By comparing and analyzing the data of the three embodiments, the following results are obtained: Example 1 changes the amount of fly ash and alkali activator relative to Example 2; Example 3 changes the amount of slag, steel slag and glass fiber added relative to Example 2. From the comparison of the test results of the embodiments, it can be obtained that the factors selected in Example 1, such as fly ash, alkali activator, steel slag, slag, glass fiber, magnesium oxide silica fume, silicone waterproofing agent, polyacrylamide, retarder, and modified resin liquid, are optimal. Relatively speaking, the compressive strength of the three embodiments is not much different. Example 1 has a faster setting time for convenient construction, a lower water absorption rate, and a strong anti-seepage ability. Compared with Example 1, Comparative Example 1 cancels the addition of modified resin liquid, and not only the compressive strength is reduced, but also the water absorption rate is greatly improved.
[0083] Most of the admixtures used in the alkali-activated fly ash of the present invention are recycled waste materials. In addition, the production energy consumption and carbon dioxide emissions of the alkali-activated technology are low, which saves energy, protects the environment, and is consistent with the green concept.
[0084] Embodiment 4:
[0085] like Figure 2 As shown, the alkali-activated fly ash compaction pile construction method of this embodiment has the following specific steps:
[0086] The vibrating pile driver method is used for drilling construction. The hole diameter is 50cm, the pile spacing is 1.2m, and the hole depth is 5m. The pile pipe should be kept vertical when driven in, with a deviation of no more than 2%.
[0087] Each pile hole is divided into 10 layers. After each layer of filler is placed in, a vibrating pile driver is used to vibrate and tamp the filled filler so that the soil layer within a certain range and depth at the bottom of the pile hole is compacted and reinforced. In this process, the first filling height is 0.5m and the number of vibration tamping is 3 times.
[0088] The second construction area is 0.5m higher than the first foundation, and a further 0.5m high filler is added to the pile hole. A vibrating pile driver is used to vibrate and tamp the filled filler. The third construction area is 0.5m higher than the second foundation, and the filler is vibrated and tamped in the same way as the first and second foundations, and the same compaction standard is used to control the degree of compaction. Repeat the above operation to complete the fourth, fifth, sixth, and... filler vibration and tamping operations, and use the same compaction standard to control the degree of compaction, and finally complete the construction of the compaction pile.
[0089] Embodiment 5:
[0090] like Figure 3 As shown, this embodiment increases the diameter of the compaction pile to 70 cm on the basis of the fourth embodiment. By increasing the diameter of the compaction pile without changing the pile spacing, the surrounding soil is more fully compacted in the compaction pile construction process, and the bearing capacity and safety are higher, which is suitable for sections with seriously insufficient foundation bearing capacity. The specific construction steps of the compaction pile are the same as those of the fourth embodiment.
[0091] Embodiment 6:
[0092] like Figure 4 As shown, the alkali-activated fly ash compaction pile construction method of this embodiment uses a pile diameter of 70 cm and a pile spacing of 1.5 m, which not only increases the pile spacing to reduce the number of piles under the same area of roadbed, but also increases the pile diameter to avoid insufficient lateral compaction due to the increase in pile spacing, which is more economical. The specific construction steps of the compaction pile are the same as those of Example 4.
[0093] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. An alkali activated fly ash grouting material, It is characterized in that The invention comprises the following raw materials in parts by weight: 480-550 parts of fly ash, 100-140 parts of alkali activator, 110-150 parts of steel slag, 100-130 parts of slag, 30-40 parts of glass fiber, 28-37 parts of magnesium oxide silica fume, 20-30 parts of organic silicon waterproofing agent, 15-22 parts of polyacrylamide, 15 parts of retarder, 10-15 parts of modified resin liquid, and the water-to-binder ratio is 0.39-0.
41.
2. The alkali-activated fly ash grouting material according to claim 1, It is characterized in that The burning content of fly ash is not more than 10%, SiO 2 +Al 2 O 3 +Fe 2 O 3 The content is greater than 60%, the particle size is controlled at 0.05-3.0mm, the fly ash fineness is not more than 30%, and the fly ash content accounts for 50%-60% of the total mass of the alkali-activated fly ash.
3. The alkali-activated fly ash grouting material according to claim 1, It is characterized in that The dosage of the alkali activator is 6%-10%, and other admixtures account for 15%-25% of the total mass.
4. The alkali-activated fly ash grouting material according to claim 1, It is characterized in that The dosage of retarder is 1%-3%.
5. A method for preparing an alkali-activated fly ash grouting material according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The raw materials of the grouting material are mixed evenly, and then put into a mixer for stirring; The uniformly stirred mixture is allowed to stand at room temperature for curing to allow the alkali-induced reaction to occur.
6. The method for preparing an alkali-activated fly ash grouting material according to claim 5, It is characterized in that The stirring speed of the stirrer is 500-600 rpm, and the stirring time is 30-40 minutes.
7. A method for constructing alkali-activated fly ash compaction piles. It is characterized in that The following steps are involved: The positions of compaction piles are arranged in an equilateral triangle; The vibrating pile driver method is used for hole construction; Filling the pile hole with filler, wherein the filler is layered and compacted on the pile top, and the filler is the alkali-activated fly ash grouting material as claimed in any one of claims 1 to 4; After filling is completed, the compacted piles are maintained.
8. The alkali-activated fly ash compaction pile construction method according to claim 7, It is characterized in that Each pile hole is divided into 5-10 layers. After each layer of filler is placed, a vibrating pile driver is used to vibrate and tamp the filler.
9. The alkali-activated fly ash compaction pile construction method according to claim 8, It is characterized in that The first filling height shall not be less than 0.5m, and the number of vibration tamping shall not be less than 3 times; Fill the pile hole with filler according to the principle that the next layer of filler should rise 0.5m-1m above the previous layer of filler.
10. The alkali-activated fly ash compaction pile construction method according to claim 7, It is characterized in that The degree of compaction is controlled by measuring the compaction degree of the filler. The compaction standard is: measuring the compaction degree after a single vibration tamping, the compaction degree change of a single vibration tamping is not greater than 2cm; or measuring the total compaction degree after three consecutive vibration tampings, the change is not greater than 5cm.