Aluminum zinc oxide target material and preparation method thereof

By pre-sintering and vacuum pressurized sintering of zinc oxide powder, the density and pore problems of zinc oxide targets are solved, the light transmittance of the film is significantly improved, and the target performance is improved.

CN118955117APending Publication Date: 2024-11-15XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410880984.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing zinc oxide aluminum target preparation methods are difficult to effectively improve the density of the target material and reduce the number of pores, resulting in insufficient light transmittance of the film.

Method used

Pre-sintering and vacuum pressurized sintering are used to improve the body density and sintering pressure, improve the density and pore size of the target material, thereby improving the sputtering effect of the film.

Benefits of technology

Through presintering and vacuum pressurized sintering technology, the density of zinc oxide aluminum target and the light transmittance of the film are significantly improved, and the performance of the target is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924497810000091
    Figure BDA0004924497810000091
  • Figure BDA0004924497810000101
    Figure BDA0004924497810000101
  • Figure BDA0004924497810000102
    Figure BDA0004924497810000102
Patent Text Reader

Abstract

The invention belongs to the field of target materials, and discloses a preparation method of an aluminum zinc oxide target material, which comprises the following steps: uniformly mixing zinc oxide powder, aluminum oxide powder, germanium oxide powder, a dispersant, a binder and pure water, and grinding to obtain first mixed slurry; adding a defoaming agent into the first mixed slurry, and stirring to obtain second mixed slurry; carrying out spray granulation, mixing and sieving on the second mixed slurry to obtain powder; pre-sintering the powder to obtain a pre-sintered body, sieving the pre-sintered body, and performing cold isostatic pressing on the pre-sintered body to obtain a green body; and finally, the obtained blank is subjected to vacuum pressure sintering, and the target material is obtained. Powder obtained through spray granulation is pre-sintered, a green body is subjected to vacuum pressure sintering, the density of the zinc aluminum oxide target material is improved, the number of internal air holes is reduced, and the transmittance of a film obtained through sputtering at the wavelength of 400-800 nm is increased; in addition, the invention also discloses the zinc aluminum oxide target material prepared by adopting the method and application of the zinc aluminum oxide target material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of target materials, and in particular to a zinc oxide aluminum target material and a preparation method thereof. Background Art

[0002] Zinc oxide aluminum target is an important functional material with excellent optical properties, electrical conductivity and chemical stability. It is widely used in optical coatings, conductive films, solar cells, display devices and other fields. The preparation technology of zinc oxide aluminum target is critical. Physical vapor deposition technology such as magnetron sputtering or electron beam evaporation is usually used to prepare zinc oxide aluminum target. During the preparation process, the composition, structure and purity of the target need to be controlled to ensure the quality and performance of the film. At the same time, the process parameters in the preparation process such as sputtering power, gas pressure, deposition rate, etc. will affect the performance of zinc oxide aluminum target.

[0003] Chinese patent application No. 200910108039.4 discloses a method for preparing a germanium-doped zinc oxide aluminum target material, the preparation method comprising: weighing raw materials of zinc oxide, aluminum oxide, and germanium oxide powder respectively in proportion, adding a binder, and mixing with water; drying the mixture by spray drying or the like, and then pressing the powder into a shape to form a blank with a predetermined shape and strength; sintering the blank at a temperature of 1200 to 1600° C. under normal pressure and atmosphere to obtain a germanium-doped zinc oxide aluminum target material.

[0004] This solution improves the density of the target material and the transmittance of the film by doping germanium oxide and adjusting the amount of germanium oxide and aluminum oxide powder added.

[0005] Chinese patent application 202110417139.6 discloses a zinc oxide aluminum target material and a preparation method thereof. The preparation method comprises the following steps of first preparing zinc oxide, aluminum oxide, a dispersant, a binder and water into a mixed slurry and defoaming the mixture; then spray granulating, mixing and screening the obtained mixed slurry to obtain zinc oxide aluminum powder; pressure molding the obtained zinc oxide aluminum powder to obtain a zinc oxide aluminum target blank; laying a layer of metal oxide powder on the bottom of the obtained zinc oxide aluminum target blank and sintering the mixture at 1300-1500°C to obtain a zinc oxide aluminum target material.

[0006] This solution significantly improves the quality of zinc oxide aluminum target by controlling the particle size and uniformity of zinc oxide aluminum powder, aluminum oxide, and zinc oxide, and improves the composition uniformity of zinc oxide aluminum target.

[0007] It is not difficult to see that the above two schemes respectively improve the performance of the target material by adjusting the amount of raw material powder added or the particle size and uniformity of the raw material powder, thereby improving the visible light transmittance of the film.

[0008] The problem that this solution needs to solve is: How to propose a new preparation method to increase the density of the target material, reduce the number of pores inside the target material, and thus improve the light transmittance of the film. Summary of the invention

[0009] To solve the above problems, the present invention provides a zinc oxide aluminum target material and a preparation method and application thereof. When the zinc oxide aluminum powder is pre-sintered once before cold isostatic pressing, the activity of the zinc oxide aluminum powder is improved, which is beneficial to the molding of the zinc oxide aluminum blank and promotes the improvement of the density of the blank. In the case of vacuum sintering, the sintering pressure is increased, the density of the target material can be improved and then the pore size can be improved, which is beneficial to improving the sputtering effect of the target material.

[0010] To achieve the above object, the present application discloses a method for preparing a zinc oxide aluminum target, comprising the following steps:

[0011] Step 1: uniformly mix zinc oxide powder, aluminum oxide powder, dopant, dispersant, binder and pure water, and grind to obtain a first mixed slurry;

[0012] Step 2: adding a defoaming agent to the first mixed slurry obtained in step 1, stirring, and obtaining a second mixed slurry;

[0013] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0014] Step 4: pre-sintering the target powder obtained in step 3 to obtain a pre-sintered body, sieving, and then hydraulically and cold isostatically pressing to obtain a green body;

[0015] Step 5: vacuum pressure sintering the green body obtained in step 4 to obtain a zinc oxide aluminum target;

[0016] The average particle size of the zinc oxide powder and the aluminum oxide powder in step 1 is 120-250 nm; the dopant is germanium oxide;

[0017] The pre-sintering temperature in step 4 is increased to 400-600°C at 1-5°C / min, and the sintering time is 2-3h;

[0018] The vacuum pressure sintering process of step 5 is: first increase the temperature to 700-900°C at 1-2°C / min, and keep it warm for 2-3 hours; continue to increase the temperature to 1200-1300°C, keep it warm for 10-15 hours, keep the temperature unchanged, start pressurizing to 50-60MPa, and keep it warm and pressurized for 3-4 hours.

[0019] Preferably, the dispersant in step 1 is at least one of polyvinyl pyrrolidone, polycarboxylic acid compounds and polyvinyl salts.

[0020] Preferably, the binder in step 1 is at least one of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salt, and polyethylene glycol.

[0021] Preferably, the defoaming agent in step 2 is at least one of polydimethylsiloxane, polyoxypropylene oxyethylene glycerol ether, and n-butanol; and the stirring time is 15 to 30 minutes.

[0022] Preferably, the mass ratio of zinc oxide powder, aluminum oxide powder and dopant in step 1 is 85-98:1-10:1-5; and the grinding time is 18-20 hours.

[0023] Preferably, the mass of the dispersant and the binder in step 1 is 1% to 5% of the total mass of the zinc oxide powder and the aluminum oxide powder; the mass of the pure water is 30% to 40% of the total mass of the zinc oxide powder and the aluminum oxide powder.

[0024] Preferably, in step 5, when the sintering pressure is 50-55 MPa, the average particle size of the zinc oxide powder is 120-200 nm (excluding 200 nm), and the average particle size of the aluminum oxide powder is 200-250 nm;

[0025] When the sintering pressure is 55 to 60 MPa (excluding 55 MPa), the average particle size of the zinc oxide powder is 200 to 250 nm, and the average particle size of the aluminum oxide powder is 120 to 200 nm (excluding 200 nm).

[0026] Preferably, the cold isostatic pressing pressure in step 4 is 350-450 MPa, and the time is 10-20 min.

[0027] In addition, the present application also discloses a zinc oxide aluminum target material obtained by using the above zinc oxide aluminum target material preparation method.

[0028] The beneficial effects of the present invention are:

[0029] The invention provides a zinc oxide aluminum target material and a preparation method thereof. The zinc oxide aluminum powder is doped with germanium oxide and spray granulated to obtain the target material powder. The target material powder is pre-sintered once to improve the activity of the zinc oxide aluminum powder, which is beneficial to the forming of the zinc oxide aluminum blank during cold isostatic pressing and has a promoting effect on improving the density of the blank. In the case of vacuum sintering, the sintering pressure is increased, the density of the target material can be improved and then the pore size can be improved, which is beneficial to improving the sputtering effect of the target material. DETAILED DESCRIPTION

[0030] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0031] Example 1

[0032] Step 1: zinc oxide powder, aluminum oxide powder, and germanium oxide powder are uniformly mixed in a mass ratio of 92:5:3, mixed with polyvinyl chloride, polyethylene glycol, and pure water, and ground for 19 hours to obtain a first mixed slurry;

[0033] Step 2: adding butanediol to the first mixed slurry obtained in step 1, stirring for 20 minutes, to obtain a second mixed slurry;

[0034] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0035] Step 4: pre-sinter the target powder obtained in step 3, the sintering temperature is increased to 500°C at 3°C / min, sintered for 2.5h to obtain a pre-sintered body, sieved, and then hydraulically pressed at a pressure of 30MPa for 20min; then cold isostatically pressed to obtain a green body;

[0036] Step 5: vacuum pressure sintering the green body obtained in step 4 to obtain a zinc oxide aluminum target;

[0037] The average particle size of the zinc oxide powder in step 1 is 225±5 nm, and the average particle size of the aluminum oxide powder is 150±5 nm;

[0038] The vacuum pressure sintering process of step 5 is as follows: first, heat to 800°C at 1.5°C / min and keep warm for 2.5 hours; then continue to heat to 1250°C and keep warm for 13 hours, keep the temperature constant, start pressurizing to 59MPa, and keep warm and pressure for 3.5 hours.

[0039] Example 2

[0040] The method is basically the same as Example 1, except that in step 1, the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder is 85:10:5.

[0041] Example 3

[0042] The method is basically the same as Example 1, except that in step 1, the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder is 98:1:1.

[0043] Example 4

[0044] It is basically the same as Example 1, except that in step 4, the pre-sintering temperature is increased to 400° C. at a rate of 1° C. / min and sintered for 2 h.

[0045] Example 5

[0046] It is basically the same as Example 1, except that in step 4, the pre-sintering temperature is increased to 600° C. at a rate of 3° C. / min and sintered for 3 h.

[0047] Example 6

[0048] It is basically the same as Example 1, except that the vacuum pressure sintering process in step 5 is: first increase the temperature to 700°C at 1°C / min and keep it warm for 2 hours; continue to increase the temperature to 1200°C and keep it warm for 10 hours, keep the temperature unchanged, start pressurizing to 50MPa, and keep it warm and pressurized for 3 hours.

[0049] Example 7

[0050] It is basically the same as Example 1, except that the vacuum pressure sintering process in step 5 is: first increase the temperature to 900°C at 2°C / min and keep it warm for 3 hours; continue to increase the temperature to 1300°C and keep it warm for 15 hours, keep the temperature unchanged, start pressurizing to 60MPa, and keep it warm and pressure for 4 hours.

[0051] Example 8

[0052] The method is substantially the same as Example 1, except that in step 1, the average particle size of the zinc oxide powder is 150±5 nm, and the average particle size of the aluminum oxide powder is 225±5 nm;

[0053] The vacuum pressure sintering process in step 5 is: first increase the temperature to 800°C at 1.5°C / min and keep it at this temperature for 2.5 hours; then continue to increase the temperature to 1250°C and keep it at this temperature for 13 hours. Then, keep the temperature constant and start pressurizing to 54MPa and keep it at this temperature and pressure for 3.5 hours.

[0054] Example 9

[0055] The method is substantially the same as Example 1, except that in step 1, the average particle size of the zinc oxide powder is 150±5 nm, and the average particle size of the aluminum oxide powder is 225±5 nm;

[0056] The vacuum pressure sintering process in step 5 is: first, heat to 800°C at 1.5°C / min and keep warm for 2.5 hours; then continue to heat to 1250°C and keep warm for 13 hours, keep the temperature unchanged, start pressurizing to 59MPa, and keep warm and pressure for 3.5 hours.

[0057] Comparative Example 1

[0058] Step 1: zinc oxide powder and aluminum oxide powder are uniformly mixed in a mass ratio of 95:5, mixed with polyvinyl chloride, polyethylene glycol and pure water, and ground for 19 hours to obtain a first mixed slurry;

[0059] Step 2: adding butanediol to the first mixed slurry obtained in step 1, stirring for 20 minutes, to obtain a second mixed slurry;

[0060] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0061] Step 4: The target powder obtained in step 3 is hydraulically pressed at a pressure of 30 MPa for 20 min; and then cold isostatically pressed to obtain a green body;

[0062] Step 5: vacuum sintering the green body obtained in step 4 under standard atmospheric pressure to obtain a zinc oxide aluminum target;

[0063] The average particle size of the zinc oxide powder in step 1 is 150±5nm, and the average particle size of the aluminum oxide powder is 225±5nm;

[0064] The vacuum pressure sintering process in step 5 is: first increase the temperature to 800°C at 1.5°C / min and keep it at this temperature for 2.5 hours; then continue to increase the temperature to 1250°C and keep it at this temperature for 13 hours, keep the temperature constant and the pressure at normal pressure, and keep the temperature and pressure at this temperature for 3.5 hours.

[0065] Comparative Example 2

[0066] Step 1: zinc oxide powder and aluminum oxide powder are uniformly mixed in a mass ratio of 92:5, mixed with polyvinyl chloride, polyethylene glycol and pure water, and ground for 19 hours to obtain a first mixed slurry;

[0067] Step 2: adding butanediol to the first mixed slurry obtained in step 1, stirring for 20 minutes, to obtain a second mixed slurry;

[0068] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0069] Step 4: pre-sinter the target powder obtained in step 3, the sintering temperature is increased to 500°C at 3°C / min, sintered for 2.5h to obtain a pre-sintered body, sieved, and then hydraulically pressed at a pressure of 30MPa for 20min; then cold isostatically pressed to obtain a green body;

[0070] Step 5: vacuum pressure sintering the green body obtained in step 4 to obtain a zinc oxide aluminum target;

[0071] The average particle size of the zinc oxide powder in step 1 is 150±5nm, and the average particle size of the aluminum oxide powder is 225±5nm;

[0072] The vacuum pressure sintering process in step 5 is: first increase the temperature to 800°C at 1.5°C / min and keep it at this temperature for 2.5 hours; then continue to increase the temperature to 1250°C and keep it at this temperature for 13 hours, and then keep the temperature constant and the pressure at 54MPa for 3.5 hours.

[0073] Comparative Example 3

[0074] Step 1: zinc oxide powder, aluminum oxide powder, and germanium oxide powder are uniformly mixed in a mass ratio of 92:5:3, mixed with polyvinyl chloride, polyethylene glycol, and pure water, and ground for 19 hours to obtain a first mixed slurry;

[0075] Step 2: adding butanediol to the first mixed slurry obtained in step 1, stirring for 20 minutes, to obtain a second mixed slurry;

[0076] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0077] Step 4: pre-sinter the target powder obtained in step 3, the sintering temperature is increased to 500°C at 3°C / min, sintered for 2.5h to obtain a pre-sintered body, sieved, and then hydraulically pressed at a pressure of 30MPa for 20min; then cold isostatically pressed to obtain a green body;

[0078] Step 5: vacuum sintering the green body obtained in step 4 under standard atmospheric pressure to obtain a zinc oxide aluminum target;

[0079] The average particle size of the zinc oxide powder in step 1 is 150±5nm, and the average particle size of the aluminum oxide powder is 225±5nm;

[0080] The vacuum pressure sintering process in step 5 is: first increase the temperature to 800°C at 1.5°C / min and keep it at this temperature for 2.5 hours; then continue to increase the temperature to 1250°C and keep it at this temperature for 13 hours, keep the temperature constant and the pressure at normal pressure, and keep the temperature and pressure at this temperature for 3.5 hours.

[0081] Comparative Example 4

[0082] Step 1: zinc oxide powder, aluminum oxide powder, and germanium oxide powder are uniformly mixed in a mass ratio of 92:5:3, mixed with polyvinyl chloride, polyethylene glycol, and pure water, and ground for 19 hours to obtain a first mixed slurry;

[0083] Step 2: adding butanediol to the first mixed slurry obtained in step 1, stirring for 20 minutes, to obtain a second mixed slurry;

[0084] Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder;

[0085] Step 4: The target powder obtained in step 3 is hydraulically pressed at a pressure of 30 MPa for 20 min; and then cold isostatically pressed to obtain a green body;

[0086] Step 5: vacuum pressure sintering the green body obtained in step 4 to obtain a zinc oxide aluminum target;

[0087] The average particle size of the zinc oxide powder in step 1 is 150±5 nm, and the average particle size of the aluminum oxide powder is 225±5 nm.

[0088] The vacuum pressure sintering process of step 5 is as follows: first, heat to 800°C at 1.5°C / min and keep warm for 2.5 hours; then continue to heat to 1250°C and keep warm for 13 hours, keep the temperature constant, start pressurizing to 54MPa, and keep warm and pressure for 3.5 hours.

[0089] Comparative Example 5

[0090] It is basically the same as Example 8, except that the dopant in step 1 is tin dioxide.

[0091] Performance Test:

[0092] The zinc oxide aluminum targets obtained in Examples 1-9 and Comparative Examples 1-4 were tested, and a coating experiment was performed. The film transmittance was tested at a light wavelength of 400-800 nm. The experimental results are shown in Table 1:

[0093] Table 1

[0094]

[0095] Result analysis:

[0096] 1. It can be seen from Examples 2-3, Example 8 and Comparative Example 2 that the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder in Example 8 is 92:5:3;

[0097] In Example 2, the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder is 85:10:5;

[0098] In Example 3, the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder is 98:1:1;

[0099] In Comparative Example 2, the mass ratio of zinc oxide powder to aluminum oxide powder is 98:1, and the properties of the prepared zinc oxide aluminum target are shown in Table 2:

[0100] Table 2

[0101]

[0102] Combined with the data in the above table, it can be seen that adding germanium oxide dopant can improve the performance of zinc oxide aluminum target, and when the mass ratio of zinc oxide powder, aluminum oxide powder and germanium oxide powder is 92:5:3, the obtained zinc oxide aluminum target has better effect.

[0103] 2. It can be seen from Example 8, Examples 4-5 and Comparative Example 4 that in Example 8 and Examples 4-5, the range of pre-sintering process parameters was optimized;

[0104] In comparative example 4, the pre-sintering process was not performed in step 4, and the properties of the prepared zinc oxide aluminum target are shown in Table 3:

[0105] Table 3

[0106]

[0107]

[0108] It can be seen from Example 8 and Comparative Example 4 that pre-sintering the target powder once can improve the activity of the zinc oxide aluminum powder, which is beneficial to the forming of the zinc oxide aluminum blank and can also increase the relative density of the blank, thereby improving the performance of the zinc oxide aluminum target.

[0109] 3. It can be seen from Examples 6-8 and Comparative Example 3 that the process parameter range of vacuum pressure sintering is optimized in Examples 6-8;

[0110] In step 5 of comparative example 3, vacuum sintering was performed under standard atmospheric pressure, and the properties of the obtained zinc oxide aluminum target are shown in Table 4:

[0111] Table 4

[0112]

[0113] It can be seen from Example 8 and Comparative Example 3 that vacuum pressure sintering in step 5 can significantly improve the relative density and transmittance of the zinc oxide aluminum target.

[0114] 4. It can be seen from Example 8 and Comparative Examples 1-4 that in Example 8, germanium oxide is added as a dopant, zinc oxide aluminum powder is pre-sintered in step 4, and vacuum pressure sintering is performed in step 5;

[0115] In Comparative Example 1, germanium oxide as a dopant was not added, the zinc oxide aluminum powder was not pre-sintered in step 4, and vacuum pressure sintering was not performed in step 5;

[0116] In comparative example 2, germanium oxide as a dopant was not added, zinc oxide aluminum powder was pre-sintered in step 4, and vacuum pressure sintering was performed in step 5;

[0117] In Comparative Example 3, germanium oxide was added as a dopant, the zinc oxide aluminum powder was pre-sintered in step 4, and vacuum pressure sintering was not performed in step 5;

[0118] In Comparative Example 4, germanium oxide was added as a dopant, the zinc oxide aluminum powder was not pre-sintered in step 4, and vacuum pressure sintering was performed in step 5. The properties of the prepared zinc oxide aluminum target are shown in Table 5:

[0119] Table 5

[0120]

[0121] It can be seen from the target performance data in the above table that adding germanium oxide as a dopant, pre-sintering the zinc oxide aluminum powder, and performing vacuum pressure sintering can improve the performance of the zinc oxide aluminum target to a certain extent; among them, vacuum pressure sintering in step 5 has the best effect on improving the zinc oxide aluminum target.

[0122] 5. It can be seen from Example 8, Example 1 and Example 9 that the average particle size of the zinc oxide powder in step 1 of Example 1 is 225±5nm, the average particle size of the aluminum oxide powder is 150±5nm, and the vacuum sintering pressure in step 5 is 59MPa;

[0123] In Example 8, the average particle size of the zinc oxide powder in step 1 is 150±5 nm, the average particle size of the aluminum oxide powder is 225±5 nm, and the vacuum sintering pressure in step 5 is 54 MPa;

[0124] In Example 9, the average particle size of the zinc oxide powder in step 1 is 150±5 nm, the average particle size of the aluminum oxide powder is 225±5 nm, and the vacuum sintering pressure in step 5 is 59 MPa;

[0125] The properties of the zinc oxide aluminum target prepared by the above process are shown in Table 6:

[0126] Table 6

[0127]

[0128] It can be seen from the experimental data that when the sintering pressure is 50-55 MPa, the average particle size of the zinc oxide powder is 120-200 nm and does not include 200 nm, and the average particle size of the aluminum oxide powder is 200-250 nm;

[0129] When the sintering pressure is 55-60 MPa but not including 55 MPa, the average particle size of the zinc oxide powder is 200-250 nm, and the average particle size of the aluminum oxide powder is 120-200 nm but not including 200 nm;

[0130] When the above two conditions are met, the prepared zinc oxide aluminum target has better performance.

[0131] 6. It can be seen from Example 8, Comparative Examples 2 and 5 that in Example 8, the added dopant is germanium oxide;

[0132] In Comparative Example 2, no dopant was added;

[0133] In Comparative Example 5, the added dopant is tin dioxide, an oxide of the same group element as germanium oxide;

[0134] The experimental data of the zinc oxide aluminum target prepared by the above process are shown in Table 7:

[0135] Table 7

[0136]

[0137] It can be seen from the experimental data that tin dioxide, as a dopant, can also improve the performance of zinc oxide aluminum target to a certain extent, but its improvement effect is far less than that of germanium oxide.

[0138] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a zinc oxide aluminum target, It is characterized in that The following steps are included: Step 1: Mix zinc oxide powder, aluminum oxide powder, a dopant, a dispersant, a binder and pure water, and grind to obtain a first mixed slurry; Step 2: adding a defoaming agent to the first mixed slurry obtained in step 1, stirring, and obtaining a second mixed slurry; Step 3: spray granulate the second mixed slurry obtained in step 2, mix and sieve to obtain target material powder; Step 4: pre-sintering the target powder obtained in step 3 to obtain a pre-sintered body, sieving, and hydraulically and cold isostatically pressing to obtain a green body; Step 5: vacuum pressure sintering the green body obtained in step 4 to obtain a zinc oxide aluminum target; The average particle size of the zinc oxide powder and the aluminum oxide powder in step 1 is 120-250 nm; the dopant is germanium oxide; The pre-sintering temperature in step 4 is increased to 400-600° C. at a rate of 1-5° C. / min, and the sintering time is 2-3 hours; The vacuum pressure sintering process of step 5 is as follows: first, heat to 700-900°C at 1-2°C / min, and keep warm for 2-3h; then continue to heat to 1200-1300°C, keep warm for 10-15h, keep the temperature unchanged, start pressurizing to 50-60MPa, and keep warm and pressure for 3-4h.

2. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The dispersant in step 1 is at least one of polyvinyl pyrrolidone, polycarboxylic acid compounds and polyvinyl salts.

3. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The binder in step 1 is at least one of polyvinyl alcohol, carboxymethyl cellulose, polyacrylamide, polyacrylic acid salt, and polyethylene glycol.

4. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The defoaming agent in step 2 is at least one of polydimethylsiloxane, polyoxypropylene oxyethylene glycerol ether, n-butanol and butanediol; and the stirring time is 15 to 30 minutes.

5. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The mass ratio of the zinc oxide powder, the aluminum oxide powder and the dopant in step 1 is 85-98:1-10:1-5; and the grinding time is 18-20 hours.

6. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The mass of the dispersant and the binder in step 1 is 1% to 5% of the total mass of the zinc oxide powder and the aluminum oxide powder; the mass of the pure water is 30% to 40% of the total mass of the zinc oxide powder and the aluminum oxide powder.

7. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that In step 5, when the sintering pressure is 50-55 MPa, the average particle size of the zinc oxide powder is 120-200 nm (excluding 200 nm), and the average particle size of the aluminum oxide powder is 200-250 nm; When the sintering pressure is 55 to 60 MPa (excluding 55 MPa), the average particle size of the zinc oxide powder is 200 to 250 nm, and the average particle size of the aluminum oxide powder is 120 to 200 nm (excluding 200 nm).

8. The method for preparing the zinc oxide aluminum target according to claim 1, It is characterized in that The cold isostatic pressing pressure in step 4 is 350-450 MPa, and the time is 10-20 min.

9. A zinc oxide aluminum target, It is characterized in that The target is prepared by the method for preparing the zinc oxide aluminum target according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Ge-doped AZO target and preparation method thereof

    CN101575207A

  • Multi-doping zinc-oxide-base wide-bandgap conducting material and preparation method thereof

    CN101661808A

  • High-density AZO target and preparation method thereof

    CN104418592A

  • Aluminum zinc oxide target material and preparation method thereof

    CN111439997A

  • Preparation method of secondary phase controllable zinc-aluminum oxide sputtering target material

    CN113149633A