High-hydrophobicity melamine resin impregnant and preparation method thereof

By combining wheat bran liquefaction products with phenol liquefaction, the water resistance and formaldehyde release problems of melamine-urea-formaldehyde resin were solved, and a modified resin with high hydrophobicity and water resistance was prepared, which increased the glue strength and reduced formaldehyde release. Provides safer and more sustainable adhesive impregnants.

CN118955833AInactive Publication Date: 2024-11-15GUANGZHOU JINGQI DECORATION MATERIALS CO LTD

Patent Information

Application Number
CN202411283651.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Melamine-urea-formaldehyde resin has poor water resistance and weather resistance, and releases harmful formaldehyde during production and use, limiting its use in certain applications.

Method used

By combining wheat bran liquefaction products with phenol liquefaction, controlling reaction conditions and adding catalysts, a modified melamine resin was prepared to reduce formaldehyde release and improve the hydrophobicity and water resistance of the resin.

Benefits of technology

The high hydrophobicity and water resistance of the modified melamine resin are achieved, which enhances the bonding strength, reduces formaldehyde emission, and provides a safer and more sustainable adhesive impregnant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042445380000021
    Figure BDA0005042445380000021
  • Figure BDA0005042445380000061
    Figure BDA0005042445380000061
  • Figure BDA0005042445380000071
    Figure BDA0005042445380000071
Patent Text Reader

Abstract

The invention discloses a high-hydrophobicity melamine resin impregnant and a preparation method thereof, and particularly belongs to the technical field of melamine modified resin. The high-hydrophobicity melamine resin impregnant is formed by compounding modified melamine resin, and the modified melamine resin is prepared from the following components: formaldehyde, urea, melamine and a wheat bran liquefied product. The preparation method of the wheat bran liquefied product comprises the following steps: adding phenol into wheat bran powder, adding concentrated sulfuric acid into the wheat bran powder, reacting for a period of time, and removing residues to obtain the wheat bran liquefied product. The modified melamine resin provided by the invention has excellent hydrophobicity, and the impregnant prepared from the modified melamine resin has good hydrophobicity and water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of melamine modified resins, and particularly relates to a modified melamine resin impregnating agent with high hydrophobicity and high water resistance and a preparation method thereof. Background Art

[0002] Melamine-urea-formaldehyde (MUF) is an amino resin synthesized by polycondensation of melamine, urea and formaldehyde. This resin is widely used in various fields such as plastic veneers, laminates, tableware, decorations and adhesives due to its good heat resistance and chemical resistance.

[0003] However, melamine-urea-formaldehyde resins also have some disadvantages. First, its water and weather resistance are relatively poor, which means that its performance may deteriorate under the influence of high humidity, ultraviolet rays or temperature changes. Second, this resin may become brittle after curing, which limits its use in certain applications that require flexibility. In addition, the production and use of melamine-urea-formaldehyde resins release formaldehyde, a hazardous substance that may pose a threat to both human health and the environment. Therefore, when using this resin, appropriate treatment is usually required to reduce the release of formaldehyde.

[0004] To overcome these shortcomings, researchers have been exploring modification methods, such as adding soy protein degradation products, liquid lignin or inorganic fillers, nanomaterials, etc. to improve its performance, including heat resistance, mechanical properties and water resistance. At the same time, by controlling the synthesis conditions such as pH value, reaction temperature and time, the performance of the resin can be optimized, its brittleness can be reduced and the release of formaldehyde can be reduced.

[0005] Despite these challenges, melamine-urea-formaldehyde resins remain important materials in many industrial applications due to their cost-effectiveness and versatility. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention aims to provide a modified melamine resin impregnating agent with high hydrophobicity and high water resistance and a preparation method thereof, thereby solving the defects of the current melamine-urea-formaldehyde resin, such as high formaldehyde content and insufficient water resistance.

[0007] In order to achieve the above object, the present invention discloses the following technical solutions:

[0008] In a first aspect, the present invention provides a modified melamine resin, which is prepared by comprising the following components in parts by mass:

[0009]

[0010] The wheat bran liquefaction product is formed by liquefying phenol.

[0011] Furthermore, the method for preparing the wheat bran liquefied product comprises the following steps:

[0012] S1. Add phenol to the bran powder, then add concentrated sulfuric acid thereto, react for 60-80 minutes to obtain a liquefied product;

[0013] S2. neutralize the liquefied product with an alkaline substance, remove the residue by centrifugal filtration, and obtain a wheat bran liquefied product.

[0014] Furthermore, the wheat bran powder is obtained by grinding and crushing dry wheat bran and then passing through a sieve with mesh size of ≥120;

[0015] In step S1, the mass ratio of phenol to wheat bran powder is (2-3):1, and the amount of concentrated sulfuric acid added is 5-8% of the mass of the wheat bran powder;

[0016] The reaction conditions are a rotation speed of 50-100 r / min and a temperature of 100-120°C.

[0017] Furthermore, the alkaline substance is at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide and zinc hydroxide.

[0018] In a second aspect, the present invention provides a method for preparing the modified melamine resin according to the first aspect, comprising the following steps:

[0019] (1) Under normal temperature conditions, a certain amount of formaldehyde is added to a reaction container, the pH value is adjusted to 8.5-9.0, and the temperature of the reaction container is raised to 50-55° C., the first part of urea and the liquefied product of wheat bran are added, and the reaction is kept warm for 30-40 minutes;

[0020] (2) then adding the first portion of melamine to the reaction vessel, raising the temperature to 90-92° C., adjusting the pH to 5.2-5.3, and reacting until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0021] (3) adjusting the pH value of the reaction mixture A to 8.0-8.5 and the temperature to 86-88° C., adding the second portion of melamine, and keeping the temperature for reaction for 1.5-2 hours;

[0022] (4) After the reaction is kept warm, the pH value is adjusted to 9.0 and the temperature is adjusted to 45° C., and the second portion of urea is added. The reaction is kept warm for 30-40 minutes to obtain a modified melamine resin.

[0023] Preferably, the mass ratio of the first part of urea to the second part of urea is 40:(5-10).

[0024] Preferably, the mass ratio of the first part of melamine to the second part of melamine is (5-7):35.

[0025] In a third aspect, the present invention provides a highly hydrophobic melamine resin impregnating agent comprising the modified melamine resin described in the first aspect.

[0026] Preferably, the highly hydrophobic melamine resin impregnating agent further comprises a curing agent and a composite filler.

[0027] Further preferably, the curing agent is an ammonium chloride solution with a concentration of ≥20wt%;

[0028] The composite filler is at least one of peanut shell powder, cooked glutinous rice powder and heavy calcium carbonate.

[0029] In the present invention:

[0030] Biomass resources are pollution-free, renewable, and easy to obtain. Therefore, the use of renewable biomass resources to prepare adhesive impregnating agents provides a sustainable development approach to alleviate many problems such as energy depletion. Wheat bran is rich in cellulose, hemicellulose, and lignin. These macromolecules in wheat bran can be degraded through liquefaction technology, providing a new idea for the preparation of adhesive impregnating agents. Phenol is used as the liquefaction medium for biomass resources. By controlling the reaction conditions and adding a catalyst (sulfuric acid), the liquefied product obtained has phenolic properties and can be directly reacted with formaldehyde to prepare an adhesive impregnating agent.

[0031] After liquefaction with phenol, the cellulose and hemicellulose in the wheat bran were degraded to varying degrees due to the interruption of ether bonds, ester bonds and carbonyl bonds, accompanied by the generation of aliphatic ethers and substances with furan structures, such as furfural or furfural derivatives. At the same time, the benzene ring on the lignin underwent a substitution reaction, indicating that the degraded lignin was cross-linked with phenol to generate a series of phenolic intermediates containing hydroxymethyl. The hydroxymethyl group, as the basic group of the chain polymerization reaction in the melamine-urea-formaldehyde system, can fully react with formaldehyde to reduce the formaldehyde content, thereby reducing formaldehyde release and improving the safety of the impregnating agent. At the same time, the liquefied wheat bran product can fully cross-link with the hydrophilic group in the melamine-urea-formaldehyde system to reduce the exposure of the hydrophilic group and achieve better hydrophobicity and water resistance.

[0032] Beneficial effects of the present invention:

[0033] The modified melamine resin provided by the present invention has excellent hydrophobicity, and the impregnating agent prepared from the modified melamine resin has good hydrophobicity and water resistance, wherein the bonding strength of the dry board can reach up to 2.13mPa, and the bonding strength after being immersed in (63±3)℃ hot water for 3h can still maintain a maximum of 2.01mPa. DETAILED DESCRIPTION

[0034] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0035] Unless otherwise specified, the test methods used in the specific implementation methods are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels; the percentages mentioned in the specific implementation methods, unless otherwise specified, are all mass percentages.

[0036] In the present invention:

[0037] Wheat bran was wheat bran purchased from Lingpan Agricultural Products Co., Ltd.;

[0038] Phenol, analytical grade, 99%, was purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0039] Concentrated sulfuric acid, analytical grade, 65%, was purchased from Guangzhou Deshu Chemical Co., Ltd.;

[0040] Sodium hydroxide, analytical grade, 99%, was purchased from Guangzhou Deshu Chemical Co., Ltd.;

[0041] Formaldehyde, analytical grade, 37%, purchased from Guangdong Qiming Chemical Technology Co., Ltd.;

[0042] Urea, analytical grade, 99%, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0043] Melamine, analytical grade, 99%, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0044] Hydrochloric acid, analytical grade, 31%, was purchased from Guangzhou Deshu Chemical Co., Ltd.

[0045] Preparation of wheat bran liquefaction product

[0046] Step (1), grinding and pulverizing the dried wheat bran, and passing through a 120-mesh sieve to obtain wheat bran powder;

[0047] Step (2), adding phenol to the wheat bran powder, wherein the mass ratio of phenol to the wheat bran powder is (2-3):1, then adding concentrated sulfuric acid with a concentration of 65wt% or more to the mixture of the two, reacting for 60-80min at a speed of 50-100r / min and heating in an oil bath to 100-120°C, wherein the amount of concentrated sulfuric acid added is 5-8% of the mass of the wheat bran powder, to obtain a liquefied product;

[0048] Step (3), cooling the liquefied product to room temperature with water, taking a certain amount of alkaline substances such as sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, and zinc hydroxide to neutralize the concentrated sulfuric acid in the wheat bran liquefied product to ensure the safety of the liquefied product, centrifuging the obtained liquefied product at high speed, filtering to remove residue, and obtaining the wheat bran liquefied product.

[0049] Preparation of Examples

[0050] Embodiment 1:

[0051] Step 1-1, under normal temperature, add 120 parts by mass of formaldehyde to a double-layer glass reactor equipped with a mechanical stirring rod, a thermometer and a condenser, take sodium hydroxide to adjust the pH value to 8.5, and heat the reaction container to 50° C., add 40 parts by mass of the first urea and 20 parts by mass of the liquefied product of wheat bran, and keep the temperature for reaction for 40 minutes;

[0052] Step 1-2, then add 5 parts by weight of melamine for the first time, raise the temperature to 90° C., add hydrochloric acid to adjust the pH to 5.2, and react until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0053] Step 1-3, adding sodium hydroxide to the reaction mixture A in step 1-2, adjusting the pH value to 8.0, cooling to 86° C., adding 35 parts by weight of melamine for the second time, and keeping the temperature for reaction for 2 hours;

[0054] Step 1-4, after the heat-keeping reaction, adjust the pH value to 9.0, and when the temperature is lowered to 45° C., add 5 parts by mass of urea for the second time, and heat-keep the reaction for 40 minutes. After the reaction is completed, the melamine-urea-formaldehyde resin modified by the liquefied product of wheat bran is obtained.

[0055] Embodiment 2:

[0056] Step 2-1, under normal temperature, add 131 parts by mass of formaldehyde to a double-layer glass reactor equipped with a mechanical stirring rod, a thermometer and a condenser, take sodium hydroxide to adjust the pH value to 9.0, and heat the reaction container to 55° C., add 40 parts by mass of the first urea and 23 parts by mass of the liquefied product of wheat bran, and keep the reaction warm for 35 minutes;

[0057] Step 2-2, then add 6 parts by mass of the first melamine, raise the temperature to 92° C., add hydrochloric acid to adjust the pH to 5.3, and react until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0058] Step 2-3, adding sodium hydroxide to the reaction mixture A in step 1-2, adjusting the pH value to 8.3, cooling to 87° C., adding 35 parts by weight of melamine for the second time, and keeping the temperature for reaction for 1.5 hours;

[0059] Step 2-4, after the heat-keeping reaction, adjust the pH value to 9.0, and when the temperature is lowered to 45° C., add 8 parts by mass of urea for the second time, and heat-keep the reaction for 30 minutes. After the reaction is completed, the melamine-urea-formaldehyde resin modified by the liquefied product of wheat bran is obtained.

[0060] Embodiment 3:

[0061] Step 3-1, under normal temperature conditions, add 140 parts by mass of formaldehyde to a double-layer glass reactor equipped with a mechanical stirring rod, a thermometer and a condenser, take sodium hydroxide to adjust the pH value to 9.0, and heat the reaction container to 55° C., add 40 parts by mass of the first urea and 25 parts by mass of the liquefied product of wheat bran, and keep the reaction warm for 30 minutes;

[0062] Step 3-2, then add 7 parts by weight of melamine for the first time, raise the temperature to 92° C., add hydrochloric acid to adjust the pH to 5.2, and react until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0063] Step 3-3, adding sodium hydroxide to the reaction mixture A in step 1-2, adjusting the pH value to 8.5, cooling to 88° C., adding 35 parts by weight of melamine for the second time, and keeping the temperature for reaction for 1.5 hours;

[0064] Step 3-4, after the heat-keeping reaction, adjust the pH value to 9.0, and when the temperature is lowered to 45°C, add 10 parts by weight of urea for the second time, and heat-keep the reaction for 30 minutes. After the reaction is completed, the melamine-urea-formaldehyde resin modified by the liquefied product of wheat bran is obtained.

[0065] Comparative Example 1:

[0066] Step 4-1, under normal temperature conditions, add 131 parts by mass of formaldehyde to a double-layer glass reactor equipped with a mechanical stirring rod, a thermometer and a condenser, take sodium hydroxide to adjust the pH value to 9.0, and heat the reaction container to 55° C., add 40 parts by mass of the first urea, and keep the reaction warm for 35 minutes;

[0067] Step 4-2, then add 6 parts by mass of melamine for the first time, raise the temperature to 92° C., add hydrochloric acid to adjust the pH to 5.3, and react until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0068] Step 4-3, adding sodium hydroxide to the reaction mixture A in step 1-2, adjusting the pH value to 8.3, cooling to 87° C., adding 35 parts by weight of melamine for the second time, and keeping the temperature for reaction for 1.5 hours;

[0069] Step 4-4, after the heat-keeping reaction, the pH value is adjusted to 9.0, and when the temperature is lowered to 45° C., 8 parts by weight of urea are added for the second time, and the heat-keeping reaction is carried out for 30 minutes. After the reaction is completed, the melamine-urea-formaldehyde resin is obtained by discharging the material.

[0070] Comparative Example 2:

[0071] Step 5-1, under normal temperature conditions, add 131 parts by mass of formaldehyde to a double-layer glass reactor equipped with a mechanical stirring rod, a thermometer and a condenser, take sodium hydroxide to adjust the pH value to 9.0, and heat the reaction container to 55° C., add 40 parts by mass of the first urea and 14 parts by mass of phenol, and keep the temperature for reaction for 35 minutes;

[0072] Step 5-2, then add 6 parts by mass of melamine for the first time, raise the temperature to 92° C., add hydrochloric acid to adjust the pH to 5.3, and react until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A;

[0073] Step 5-3, adding sodium hydroxide to the reaction mixture A in step 1-2, adjusting the pH value to 8.3, cooling to 87° C., adding 35 parts by weight of melamine for the second time, and keeping the temperature for reaction for 1.5 hours;

[0074] Step 5-4, after the heat-keeping reaction, the pH value is adjusted to 9.0, and when the temperature is lowered to 45° C., 8 parts by mass of urea are added for the second time, and the heat-keeping reaction is carried out for 30 minutes. After the reaction is completed, phenol-melamine-urea-formaldehyde resin is obtained by discharging the material.

[0075] The specific raw material weight parts and preparation parameters of the above examples and comparative examples are shown in Table 1.

[0076] Table 1 Preparation materials and parameters of resins in Examples and Comparative Examples

[0077]

[0078]

[0079] Note: “-” in the table means not added.

[0080] Performance Test:

[0081] A certain amount of ammonium chloride is dissolved in water to prepare a 20wt% ammonium chloride aqueous solution as a curing agent. The resins prepared in Examples 1-3 and Comparative Examples 1 and 2 are mixed with the curing agent (the addition amount is 2% of the resin mass) respectively, and a composite filler (the composite filler components are peanut shell powder, cooked glutinous rice flour, and heavy calcium carbonate, the mass ratio of which is 6:2.5:1.5, and the addition amount is 10% of the mass of the adhesive impregnating agent) is added to adjust the viscosity. The obtained resin impregnating agent is used to prepare a three-layer plywood, the veneer is poplar wood, the thickness is 1.5mm, the moisture content is 8-10%, and the glue coating amount is 300g / m 2 , double-sided adhesive coating, hot pressing process with a pressure of 1.0mPa / m 2 , temperature 130℃, time 10min.

[0082] Test plan: Prepare three-layer plywood according to the above process, and test the dry and wet bonding strength of plywood according to GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels". The wet bonding strength is tested according to the test method for Class II plywood, that is, immerse the specimen in hot water at (63±3)℃ for 3h, take it out and cool it at room temperature for 10min.

[0083] The performance test results of Examples 1-3 and Comparative Examples 1 and 2 are shown in Table 2.

[0084] Table 2 Plywood bonding strength test results

[0085] Group\Test Item Dry bonding strength / mPa Wet bonding strength / mPa Example 1 2.10 1.96 Example 2 2.13 2.01 Example 3 2.06 1.93 Comparative Example 1 2.11 Glue opening Comparative Example 2 1.96 0.76

[0086] Result analysis:

[0087] It can be seen from Table 2 above that the plywood prepared in Examples 1-3 has a relatively high dry board bonding strength, which can reach up to 2.13 mPa, and the bonding strength after being immersed in (63±3)°C hot water for 3 hours can still be maintained at a maximum of 2.01 mPa, indicating that the impregnating agent prepared by the present invention has good hydrophobicity and water resistance.

[0088] Finally, it should be noted that the above embodiments and comparative examples are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A modified melamine resin, characterized in that: The composition comprises the following components by weight: The wheat bran liquefaction product is formed by liquefying phenol.

2. The modified melamine resin according to claim 1, characterized in that The preparation method of the wheat bran liquefied product comprises the following steps: S1. Add phenol to the bran powder, then add concentrated sulfuric acid thereto, react for 60-80 minutes to obtain a liquefied product; S2. neutralize the liquefied product with an alkaline substance, remove the residue by centrifugal filtration, and obtain a wheat bran liquefied product.

3. The modified melamine resin according to claim 2, characterized in that The wheat bran powder is prepared by grinding and crushing dry wheat bran and then passing through a sieve with mesh size of ≥120; In step S1, the mass ratio of phenol to wheat bran powder is (2-3):1, and the amount of concentrated sulfuric acid added is 5-8% of the mass of the wheat bran powder; The reaction conditions are a rotation speed of 50-100 r / min and a temperature of 100-120°C.

4. The modified melamine resin according to claim 2, characterized in that The alkaline substance is at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide and zinc hydroxide.

5. The method for preparing the modified melamine resin according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Under normal temperature conditions, a certain amount of formaldehyde is added to a reaction container, the pH value is adjusted to 8.5-9.0, and the temperature of the reaction container is raised to 50-55° C., the first part of urea and the liquefied product of wheat bran are added, and the reaction is kept warm for 30-40 minutes; (2) then adding the first portion of melamine to the reaction vessel, raising the temperature to 90-92° C., adjusting the pH to 5.2-5.3, and reacting until the viscosity reaches 90-100 mPa·s to obtain a reaction mixture A; (3) adjusting the pH value of the reaction mixture A to 8.0-8.5 and the temperature to 86-88° C., adding the second portion of melamine, and keeping the temperature for reaction for 1.5-2 hours; (4) After the reaction is kept warm, the pH value is adjusted to 9.0 and the temperature is adjusted to 45° C., and the second portion of urea is added. The reaction is kept warm for 30-40 minutes to obtain a modified melamine resin.

6. The method for preparing the modified melamine resin according to claim 5, characterized in that: The mass ratio of the first part of urea to the second part of urea is 40:(5-10).

7. The method for preparing the modified melamine resin according to claim 5, characterized in that: The mass ratio of the first part of melamine to the second part of melamine is (5-7):

35.

8. A highly hydrophobic melamine resin impregnating agent, characterized in that: The invention comprises the modified melamine resin according to any one of claims 1 to 4.

9. The highly hydrophobic melamine resin impregnating agent according to claim 8, characterized in that: It also contains a curing agent and a composite filler.

10. The highly hydrophobic melamine resin impregnating agent according to claim 9, characterized in that: The curing agent is an ammonium chloride solution with a concentration of ≥20wt%; The composite filler is at least one of peanut shell powder, cooked glutinous rice powder and heavy calcium carbonate.

Citation Information

Patent Citations

  • Preparation method of modified biomass liquefaction resin adhesive with high water resistance

    CN104130733A

  • Melamine-urea-formaldehyde copolycondensation resin adhesive for laminated wood and preparation method thereof

    CN104893633A

  • Degradable material as well as preparation method and application thereof

    CN114231047A

  • Modified melamine adhesive and preparation method thereof

    CN116355563A

  • Multi-enzyme and multi-steps type method for producing diet cellulose flour from wheat bran

    CN1718107A

Cited By

  • Waterproof environment-friendly melamine-urea resin impregnant as well as preparation method and application thereof

    CN120921484A

  • A waterproof and environmentally friendly melamine-urea-formaldehyde resin impregnating agent, its preparation method and application