Synthesis method and application of adsorption material for extracting lithium based on tetraoxacycloalkene

The lithium-extracting adsorbent materials with high specific surface area and stability were prepared by porous organic polymers based on tetraoxycycloene, which solved the problem of insufficient specific surface area and stability of existing lithium-ion adsorbent materials, and achieved the goal of realizing the problem of insufficient specific surface area and stability of existing lithium-ion adsorbent materials. It has efficient and environmentally friendly lithium ion extraction effect.

CN118955877APending Publication Date: 2024-11-15SHENZHEN DIBO ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411042794.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium-ion adsorption materials have insufficient specific surface area and stability, resulting in limited lithium-ion adsorption capacity, low extraction efficiency and purity in complex environments, and the organic stabilizer used in the modification process increases the cost and The environment causes pollution.

Method used

Using porous organic polymers based on tetraoxycycloene, lithium-extracting adsorbent materials with clear hollow layered planar structures are prepared through specific synthetic methods, using high specific surface area and specific functional groups to provide a large number of adsorption points and at high temperatures Covalent bonds are formed under to improve stability.

Benefits of technology

It significantly improves the adsorption capacity and selectivity of lithium ions, enhances the extraction efficiency and purity in complex salt lake environments, and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955877A_ABST
    Figure CN118955877A_ABST
Patent Text Reader

Abstract

The invention discloses an adsorption material for extracting lithium based on tetraoxacycloalkene, which is composed of tetraoxa [8] cycloalkene repetitive structure units, has a clearly hollowed layered plane structure, and contains a 24-crown 4 permanent porous organic polymer. The synthesis method of the adsorbing material comprises the following steps: firstly, putting a 1, 4, 5, 8-anthraquinone monomer into a reaction system, and adding an auxiliary agent and a catalyst; then vacuumizing, standing, heating and carrying out polymerization reaction; after the reaction is finished, cooling to room temperature, stirring, slurrying and dispersing, carrying out liquid-solid separation, and washing; and finally carrying out vacuum drying to obtain the lithium extraction adsorption material based on tetraoxacycloalkene. The adsorption material serves as a novel lithium extraction adsorption material, the lithium ion adsorption capacity can reach 37.3 mg / g, the adsorption material is remarkably superior to an existing lithium extraction adsorbent, and the adsorption material has high stability and weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a synthesis method of a tetraoxocyclopentene-based lithium-extraction adsorption material and application of the prepared adsorption material, belonging to the technical field of polymer materials. Background Art

[0002] Common methods for recovering lithium from brine include solvent extraction, precipitation crystallization, adsorption, membrane separation, etc. The adsorption method has developed rapidly in recent years due to its outstanding advantages such as low cost, simple operation, green environmental protection, high selectivity and wide application range. Obviously, the adsorption material is the core of lithium extraction by adsorption.

[0003] At present, adsorption materials can be roughly divided into organic, inorganic and composite adsorption materials. Organic adsorption materials mainly include crown ethers, calixarene, etc., inorganic adsorption materials mainly include aluminum-based adsorbents, lithium ion sieves, natural minerals and carbon materials, etc. Composite adsorption materials are formed by grafting or polymerizing crown ethers, calixarene, etc. onto matrices such as fibers, organic resins, and porous macromolecular materials to form organic ligand composite adsorption materials. Crown ethers are expensive and difficult to recycle, and calixarene is not easy to dissolve and coordinate. Inorganic adsorption materials have fixed structures and chemical compositions, and their pore sizes and surface properties are difficult to precisely control. Composite adsorption materials have relatively low specific surface areas, and effective lithium ion adsorption sites are buried. The lithium ion adsorption capacity per unit volume or unit mass is limited. In the synthesis process, environmentally harmful components or difficult-to-degrade chemicals are introduced, causing potential pollution to the environment.

[0004] In recent years, some studies have attempted to improve the intrinsic adsorption capacity of inorganic structures by mixing organic units into adsorbents. For example, Chinese patent CN202410130247.9 attempts to use manganese, aluminum, and titanium powder inorganic adsorbents in the presence of organic stabilizers (essentially surfactants) and polyoxymethylene and crown ethers to blend. The resulting adsorbent has an adsorption capacity of up to 12.49 mg / g for lithium ions. After 20 cycles of adsorption-analysis experiments, the adsorption rate and analysis rate can be stabilized between 87% to 88% and 95% to 98%. Although this modification method does improve the adsorption and analysis capabilities of inorganic adsorbents, there are still some problems and limitations in its essence. First, the modification method mainly relies on surface modification and blending. The essence of the modification does not effectively increase the specific surface area of ​​the adsorption unit. High specific surface area is the key to achieving high adsorption capacity. Only by significantly increasing the specific surface area can more adsorption sites be provided. Secondly, after 20 cycles in the adsorption-desorption experiment, the adsorption rate and desorption rate can still be maintained at a high level, but the stability and economy of long-term and multiple cycles still need to be further evaluated. Finally, the organic stabilizers and other additives used in the modification process increase costs and impose a greater burden on the environment.

[0005] Porous organic polymers (POPs) and covalent organic frameworks (COFs) are materials with permanent porosity, chemical and structural tunability, and charge transport potential. In recent years, these materials have shown significant advantages in the field of lithium extraction from salt lakes. POP and COF materials achieve efficient and selective adsorption of lithium ions through their high specific surface area, porosity, and specific functionalization. Their stability and durability enable them to perform well in the complex environment of salt lakes, and through specific applications such as adsorption-desorption, electrochemical lithium extraction, and membrane separation technology, they significantly improve the efficiency and economy of lithium ion extraction. These characteristics make POP and COF materials a very promising choice in the process of lithium extraction from salt lakes.

[0006] Tetracycline polymer (pTOC) is a new type of porous semiconductor material with a high specific surface area. It combines the unique electronic properties of tetracycline (TOC) and the structural advantages of polymers, showing efficient adsorption capacity, light switchability and excellent semiconductor properties, and has broad application prospects in many fields. With the advancement of synthesis technology and in-depth research on its properties, the development and application of pTOC will promote the development of efficient, environmentally friendly and economical lithium extraction processes, providing strong technical support for the future utilization of lithium resources. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a new porous lithium adsorption material.

[0008] Another object of the present invention is to provide a method for synthesizing the novel porous lithium adsorption material.

[0009] Another object of the present invention is to provide the novel porous lithium adsorption material for use in separating and enriching lithium ions in salt lake brine.

[0010] In order to solve the above problems, the present invention provides a tetraoxacycloolefin-based lithium adsorption material, which is composed of the following tetraoxa[8]cycloolefin repeating structural units:

[0011]

[0012] The lithium extraction adsorption material has a clearly hollowed-out layered planar structure and is a permanent porous organic polymer containing 24-crown-4.

[0013]

[0014] The above-mentioned tetraoxocyclopentene-based lithium adsorption material is prepared by the following synthesis method, which comprises the following steps:

[0015] A) placing 1,4,5,8-anthraquinone monomer in a reaction system, adding 2 to 3 times the amount of the monomer substance as an auxiliary agent and 2 to 4 times the amount of the catalyst to obtain a reaction mixture;

[0016] B) evacuating the reaction system to maintain the internal pressure at 0.05 atm to 0.2 atm, and then heating the reaction mixture to perform a polymerization reaction at 250° C. to 350° C. for 100 to 150 hours to obtain a black solid;

[0017] C) After the reaction is completed, the reaction mixture is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixture of water and methanol in a volume ratio of 1:1, and the mixture is stirred and slurried for 10 h to 22 h, and the solid is separated by liquid-solid separation, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;

[0018] D) The washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxadiene-based lithium adsorption material.

[0019] In step B, the reaction temperature is maintained at 250°C to 350°C, preferably 300°C to 350°C. In this temperature range, the reaction mixture is in a semi-molten state, which improves the reaction efficiency, ensures the precisely designed target product structure, and increases the adsorption capacity for lithium ions.

[0020] The reaction mixture in step A also contains an activator in an amount of 1 to 1.5 times the amount of the monomer substance, including methanesulfonic acid and trifluoromethanesulfonic acid. The activator significantly improves the reaction efficiency, reduces the activation energy of the reaction, and further ensures the precisely designed target product structure and the ability to capture lithium ions.

[0021] The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.

[0022] The catalyst in step A comprises titanium chloride, aluminum chloride, iron chloride, zinc chloride or a mixture thereof.

[0023] The tetraoxocyclopentane-based lithium adsorption material prepared by the above-mentioned synthesis method is used to separate and enrich lithium ions in salt lake brine.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The tetraoxocyclopentene lithium adsorption material of the present invention is a new type of lithium extraction adsorption material, and its lithium ion adsorption capacity can reach 37.3 mg / g, which is significantly better than the existing lithium extraction adsorbents. The tetraoxocyclopentene lithium extraction adsorption material of the present invention is composed of tetraoxa[8]cyclopentene repeating structural units, has a clearly hollowed-out layered planar structure, and is a permanent porous organic polymer containing 24 crown 4. This structure has an extremely high specific surface area and specific functional groups, and can provide a large number of effective lithium ion adsorption sites. On the other hand, this structure also greatly improves the selectivity of the tetraoxocyclopentene lithium extraction adsorption material for lithium ions, while also reducing the interference of other ions. In a complex salt lake environment, it can effectively improve the purity and efficiency of lithium ion extraction.

[0026] 2. The present invention is based on the synthesis of tetraoxocycloolefin lithium adsorption materials at extremely high temperatures, and the covalent bond binding energy is extremely high. Compared with existing lithium adsorption materials, it has higher stability and tolerance to high salinity and extreme chemical environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a chemical structure diagram of the tetraoxacyclopentene structural unit;

[0028] Figure 2 Chemical structure of tetraoxocyclopentene lithium adsorption material

[0029] Figure 3 This is the NMR C spectrum of tetraoxocyclopentene lithium adsorption material;

[0030] Figure 4 This is the XRD spectrum of tetraoxocycloolefin lithium adsorption material;

[0031] Figure 5 This is the SEM spectrum of tetraoxocycloolefin lithium adsorption material. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known knowledge and technology is omitted to avoid unnecessary confusion of the concept of the present invention.

[0033] The present invention provides a tetraoxocyclopentane-based lithium adsorption material, such as Figure 1 , Figure 2 The lithium extraction adsorption material has a clear hollow layered planar structure and is a permanent porous organic polymer containing 24 crown 4.

[0034] The above-mentioned tetraoxocyclopentene-based lithium adsorption material is prepared by the following synthesis method, which comprises the following steps:

[0035] A) placing 1,4,5,8-anthraquinone monomer in a reaction system, adding 2 to 3 times the amount of the monomer substance as an auxiliary agent and 2 to 4 times the amount of the catalyst to obtain a reaction mixture;

[0036] B) evacuating the reaction system to maintain the internal pressure at 0.05 atm to 0.2 atm, and then heating the reaction mixture to perform a polymerization reaction at 250° C. to 350° C. for 100 to 150 hours to obtain a black solid;

[0037] C) After the reaction is completed, the reaction mixture is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixture of water and methanol in a volume ratio of 1:1, and the mixture is stirred and slurried for 10 h to 22 h, and the solid is separated by liquid-solid separation, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer;

[0038] D) The washed target polymer is vacuum dried at 80° C. to 82° C. to obtain a tetraoxadiene-based lithium adsorption material.

[0039] Figure 3 This is the NMR C spectrum of tetraoxocyclopentene lithium adsorption material.

[0040] Figure 4 This is the XRD spectrum of tetraoxocycloolefin lithium adsorption material.

[0041] Figure 5 This is the SEM spectrum of tetraoxocycloolefin lithium adsorption material.

[0042] In step B, the reaction temperature is maintained at 250°C to 350°C, preferably 300°C to 350°C. In this temperature range, the reaction mixture is in a semi-molten state, which improves the reaction efficiency, ensures the precisely designed target product structure, and increases the adsorption capacity for lithium ions.

[0043] The reaction mixture in step A also contains an activator in an amount of 1 to 1.5 times the amount of the monomer substance, including methanesulfonic acid and trifluoromethanesulfonic acid. The activator significantly improves the reaction efficiency, reduces the activation energy of the reaction, and further ensures the precisely designed target product structure and the ability to capture lithium ions.

[0044] The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.

[0045] The catalyst in step A comprises titanium chloride, aluminum chloride, iron chloride, zinc chloride or a mixture thereof.

[0046] Some examples of the synthesis of tetraoxacycloolefin-based lithium adsorption materials are listed below.

[0047]

Example 1

[0048] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0049] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 1 times the amount of sodium chloride and 1 times the amount of potassium chloride, as well as 2 times the amount of aluminum chloride, are added to obtain a reaction mixture; then, vacuum is evacuated, and the internal pressure of the reaction system is maintained at 0.1 atm and allowed to stand for 2 hours, and the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 250° C. for 100 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, and the mixture is stirred and slurried for 10 hours, liquid-solid separation is performed, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0050]

Example 2

[0051] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0052] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 1 times the amount of sodium chloride and 1 times the amount of potassium chloride, as well as 2 times the amount of aluminum chloride, are added to obtain a reaction mixture; then, vacuum is evacuated, the internal pressure of the reaction system is maintained at 0.1 atm and the reaction is allowed to stand for 2 hours, the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 300° C. for 100 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 10 hours, liquid-solid separation is performed, and the target polymer is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0053]

Example 3

[0054] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0055] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 1 times of sodium chloride and 1 times of potassium chloride, 2 times of aluminum chloride and 1 times of methanesulfonic acid are added to obtain a reaction mixture; then, vacuum is evacuated, and the internal pressure of the reaction system is maintained at 0.1 atm and allowed to stand for 2 hours, and the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 300° C. for 100 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 10 hours, liquid-solid separation is performed, and the mobile phase is methanol, pyridine, tetrahydrofuran and water are used to wash in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0056]

Example 4

[0057] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0058] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 3 times the amount of sodium chloride, 2 times the amount of zinc chloride, 2 times the amount of ferric chloride and 1.5 times the amount of methanesulfonic acid are added to obtain a reaction mixture; then, vacuum is evacuated, and the internal pressure of the reaction system is maintained at 0.05 atm and allowed to stand for 1.5 hours, and the reaction mixture is heated to carry out a polymerization reaction, and the reaction is maintained at 350° C. for 120 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 18 hours, liquid-solid separation is performed, and the mobile phase is methanol, pyridine, tetrahydrofuran and water are used to wash in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0059]

Example 5

[0060] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0061] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 2 times the amount of potassium chloride, 1 times the amount of magnesium chloride, 3 times the amount of titanium chloride and 1 times the amount of trifluoromethanesulfonic acid are added to obtain a reaction mixture; then, vacuum is evacuated, the internal pressure of the reaction system is maintained at 0.15 atm and the reaction is allowed to stand for 2.0 hours, the reaction mixture is heated to carry out a polymerization reaction, and the reaction is maintained at 320° C. for 150 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 22 hours, liquid-solid separation is performed, and the mobile phase is methanol, pyridine, tetrahydrofuran and water are used to wash in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0062]

Example 6

[0063] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0064] First, 1.0 mol of 1,4,5,8-anthraquinone monomer is placed in a reaction system, and 1 times the amount of magnesium chloride, 1 times the amount of calcium chloride, 1.5 times the amount of zinc chloride, 1.5 times the amount of titanium chloride and 1.5 times the amount of trifluoromethanesulfonic acid are added to obtain a reaction mixture; then, vacuum is evacuated, and the internal pressure of the reaction system is maintained at 0.2 atm and allowed to stand for 2.5 hours, and the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 300° C. for 130 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 16 hours, liquid-solid separation is performed, and the mobile phase is methanol, pyridine, tetrahydrofuran and water are used to wash in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0065] [Comparative Example 1]

[0066] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0067] First, 0.5 mol of 1,4-anthraquinone and 0.5 mol of 1,4,5,8-anthraquinone mixed monomers are placed in a reaction system, and 1 times the amount of sodium chloride and 1 times the amount of potassium chloride, as well as 2 times the amount of aluminum chloride, are added to the monomer substance to obtain a reaction mixture; then, vacuum is evacuated, the internal pressure of the reaction system is maintained at 0.1 atm and allowed to stand for 2 hours, the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 250° C. for 100 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 10 hours, liquid-solid separation is performed, and the target polymer is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocyclopentene-based lithium extraction adsorption material.

[0068] [Comparative Example 2]

[0069] Synthesis method of lithium adsorption material based on tetraoxacyclopentane

[0070] First, 0.5 mol of 1,4-naphthoquinone and 0.5 mol of 1,4,5,8-anthraquinone mixed monomers are placed in a reaction system, and 1 times the amount of sodium chloride and 1 times the amount of potassium chloride, as well as 2 times the amount of aluminum chloride, are added to the monomer substance to obtain a reaction mixture; then, vacuum is evacuated, the internal pressure of the reaction system is maintained at 0.1 atm and allowed to stand for 2 hours, the reaction mixture is heated to carry out a polymerization reaction, and the reaction temperature is maintained at 250° C. for 100 hours to obtain a black solid; after the reaction is completed, it is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixed solution of water and methanol in a volume ratio of 1:1, stirred and slurried for 10 hours, liquid-solid separation is performed, and the target polymer is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in turn to obtain a target polymer; finally, the washed target polymer is vacuum dried at 80° C. to 83° C. to obtain a tetraoxocycloene-based lithium extraction adsorption material.

[0071] [Comparative Example 3]

[0072] Preparation of conventional unmodified aluminum-based adsorbent by coprecipitation method

[0073] First, 0.5 mol LiCl and 1.0 mol AlCl3 were weighed and placed in 100 ml water, and mixed and dissolved completely to obtain a lithium aluminum aqueous solution; then, 20 ml of a 6 mol / L NaOH solution was prepared and heated to 80°C; the lithium aluminum aqueous solution was then added dropwise to the high-speed stirred NaOH solution at a stirring speed of 350 rpm, and the temperature was maintained at 80°C for a full reaction of 1 hour, and a solid precipitate was obtained by vacuum distillation, which was then washed with distilled water for several times and freeze-dried to obtain [LiAl2(OH)6]X n- 1-n mH2O aluminum-based adsorbent.

[0074] [Simulation test of lithium extraction from salt lake]

[0075] Simulated salt lake brine: Na + 98.01g / L, Mg 2+ 17.1g / L, Li + 0.78g / L, Cl - 191.3g / L, Ca 2+ 0.12g / L, K + 16.7g / L, SO4 2- 21.9g / L, pH 7.24.

[0076] Test method:

[0077] The adsorbent materials were placed in a group of simulated salt lake brine (pre-adsorption solution) and stirred for adsorption at a temperature of 15°C, a stirring speed of 300 r / min, and an adsorption time of 2 h. After the adsorption was completed, vacuum filtration was performed to obtain the post-adsorption solution and the loaded adsorbent material.

[0078] Take the above-mentioned loaded adsorbent material, and desorb it with a hydrochloric acid solution with a concentration of 0.5 mol / L at a rotation speed of 300 r / min and a desorption time of 2 h. After the desorption is completed, vacuum filtration is performed to obtain a desorption solution and an unloaded adsorbent material.

[0079] The element concentrations in the solution before adsorption, the solution after adsorption and the desorption solution were determined by ICP-MS.

[0080] The adsorption capacity of the adsorbent material for lithium ions is calculated according to the following formula:

[0081] Q t =(C0-C t )×V / m

[0082] Among them, Q t ——Adsorption capacity, C0——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorption material.

[0083] The tetraoxacyclopentene-based lithium extraction adsorption materials obtained in Examples 1 to 6 and the adsorption materials obtained in Comparative Examples 1 to 3 were used to conduct a salt lake lithium extraction simulation test. The test results are shown in Table 1.

[0084] Table 1 Adsorption capacity of adsorbent materials for lithium ions, mg / g

[0085]

[0086] Test conclusion:

[0087] 1. The tetraoxocyclopentene lithium adsorption material of the present invention is a new type of lithium extraction adsorption material, and its lithium ion adsorption capacity can reach 37.3 mg / g, which is significantly better than the existing lithium extraction adsorbents. The tetraoxocyclopentene lithium extraction adsorption material of the present invention is composed of tetraoxa[8]cyclopentene repeating structural units, has a clearly hollowed-out layered planar structure, and is a permanent porous organic polymer containing 24 crown 4. This structure has an extremely high specific surface area and specific functional groups, and can provide a large number of effective lithium ion adsorption sites. On the other hand, this structure also greatly improves the selectivity of the tetraoxocyclopentene lithium extraction adsorption material for lithium ions, while also reducing the interference of other ions. In a complex salt lake environment, it can effectively improve the purity and efficiency of lithium ion extraction.

[0088] 2. The present invention is based on the synthesis of tetraoxocycloolefin lithium adsorption materials at extremely high temperatures, and the covalent bond binding energy is extremely high. Compared with existing lithium adsorption materials, it has higher stability and tolerance to high salinity and extreme chemical environments.

[0089] 3. The present invention is based on the synthesis method of tetraoxocycloolefin lithium adsorption material. The selection of monomers, reaction temperature range and activator has a great influence on the reaction efficiency. Appropriate conditions can ensure the precisely designed target product structure, thereby improving the adsorption capacity of lithium ions.

[0090] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for synthesizing a lithium adsorption material based on tetraoxocyclopentane, characterized in that: The following steps are included: A) placing a 1,4,5,8-anthraquinone monomer in a reaction system, adding an auxiliary agent of 2 to 3 times the amount of the monomer substance and a catalyst of 2 to 4 times the amount of the monomer substance, to obtain a reaction mixture; B) evacuating the reaction system to maintain the internal pressure at 0.05 atm to 0.2 atm, and then heating the reaction mixture to perform a polymerization reaction at 250° C. to 350° C. for 100 to 150 hours to obtain a black solid; C) After the reaction is completed, the reaction mixture is cooled to room temperature, and the obtained black solid is acidified by adding 2N hydrochloric acid to a mixture of water and methanol in a volume ratio of 1:1, and the mixture is stirred and slurried for 10 h to 22 h, and the solid is separated by liquid-solid separation, and the mixture is washed with mobile phases of methanol, pyridine, tetrahydrofuran and water in sequence to obtain the target polymer; D) vacuum drying the washed target polymer at 80° C. to 82° C. to obtain the tetraoxadiene-based lithium adsorption material.

2. The method for synthesizing a tetraoxocyclopentane-based lithium adsorption material according to claim 1, characterized in that: Step B is carried out at 250°C to 350°C, preferably 300°C to 350°C.

3. The synthesis method of tetraoxocyclopentane-based lithium adsorption material according to claim 2, characterized in that: In step A, the reaction mixture further comprises an activator in an amount 1 to 1.5 times the amount of the monomer substance, and the activator comprises methanesulfonic acid and trifluoromethanesulfonic acid.

4. The method for synthesizing a tetraoxocyclopentane-based lithium adsorption material according to any one of claims 1 to 3, characterized in that: The auxiliary agent in step A includes sodium chloride, potassium chloride, magnesium chloride, calcium chloride or a mixture thereof.

5. The method for synthesizing a tetraoxocyclopentane-based lithium adsorption material according to any one of claims 1 to 3, characterized in that: The catalyst in step A comprises titanium chloride, aluminum chloride, iron chloride, zinc chloride or a mixture thereof.

6. A tetraoxadiene-based lithium adsorption material prepared by the synthesis method according to claims 1 to 5, characterized in that: The tetraoxacycloolefin-based lithium adsorption material is composed of the following tetraoxa[8]cycloolefin repeating structural units: The following well-defined hollowed-out layered planar structure is formed, comprising 24 crowns 4 of a permanently porous organic polymer.

7. The tetraoxocyclopentane-based lithium adsorption material according to claim 6 is used to separate and enrich lithium ions in salt lake brine.