BOPP (biaxially-oriented polypropylene) water-based acrylic acid coated anti-wrinkle cigarette packaging film and preparation method thereof
By using the external and internal coating structure on the BOPP film, and using materials such as acrylate emulsions, multi-copolymer emulsions and PVDC emulsions, the problems of surface tension and adhesion wrinkles of BOPP film are solved, and the film's anti-photoaging and barrier are improved Performance, achieving low temperature heat sealing and moisture-proof effects.
Patent Information
- Application Number
- CN202411034280.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The surface tension of the existing BOPP coating film drops rapidly, easily sticks and wrinkles, affecting the sealing quality of the cigarette and the aesthetics of the outer packaging.
BOPP aqueous acrylic-coated anti-wrinkle smoke packaging film including an outer coating film layer, a BOPP base layer and an inner coating film layer. The outer coating film layer material consists of acrylic emulsion, a multi-copolymer emulsion and polyvinyl alcohol, and the inner coating film layer material is It consists of acrylate emulsion, PVDC emulsion and polyether modified heptamethyl trisiloxane to improve the photoaging, wear resistance and barrier properties of the film through specific ratios and process treatments.
Effectively improve the photoaging, wear resistance and barrier properties of BOPP film, solve the problems of surface tension reduction, adhesion and wrinkling, and achieve excellent low-temperature heat sealing performance, strong moisture-proof barrier properties, high transparency and good printing properties. effect.
Smart Images

Figure BDA0004970650490000081 
Figure BDA0004970650490000082 
Figure BDA0004970650490000091
Abstract
Description
Technical Field
[0001] The invention relates to a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film and a preparation method thereof, belonging to the field of BOPP pre-coated cigarette films. Background Art
[0002] The inherent characteristics of BOPP coating film make it widely used in the soft packaging industry, such as cigarette labels, laser, food packaging, etc. At present, cigarettes at home and abroad are packaged in two forms: soft packs and hard boxes. In order to prevent cigarettes from getting damp and extend the shelf life of the product, the outer packaging is usually covered with a layer of BOPP ordinary film or shrink film after the strip box label paper. With the new requirements of reducing costs put forward by the cigarette industry, the cigarette industry proposes to remove the outer layer of strip box label paper and directly use BOPP coating film instead.
[0003] The existing BOPP coated film has the following shortcomings: due to the characteristics of BOPP, the surface of the BOPP coated film is non-polar, and the surface tension generally does not exceed 32 dynes, which decreases very quickly, and the coating is uneven. When used in the cigarette machine later, the seal is prone to wrinkling, causing the seal to rupture, affecting the later storage of cigarettes; directly using BOPP coated film for outer packaging will adhere to the BOPP ordinary film or shrink film for the outer packaging of the small box during the cigarette machine packaging process; BOPP coated film is prone to wrinkling after being sealed and hot-stamped by the cigarette machine, making the outer packaging of the strip box unable to achieve a delicate and beautiful effect, which has put higher and higher requirements on the heat resistance, shrinkage and machine adaptability of BOPP coated film. Summary of the invention
[0004] The invention provides a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film and a preparation method thereof, which solves the problems of fast drop in surface tension, easy adhesion and wrinkling of the existing BOPP cigarette film.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0006] A BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film, comprising an outer coating layer, a BOPP base layer and an inner coating layer;
[0007] The material of the outer coating layer includes, by weight percentage, 10-15% acrylic emulsion, 3-5% multi-polymer emulsion, 1-2% polyvinyl alcohol, 0.3-0.5% leveling agent, and the balance is solvent;
[0008] The material of the BOPP base layer includes, by weight percentage, 75-80% of propylene-butadiene copolymerized polypropylene, 10-15% of metallocene polypropylene, 3-5% of ethylene-propylene-butadiene terpolymer, 0.5-1% of antioxidant, 2-3% of compatibilizer, 0.5-1% of lubricant, and 2-2.3% of adhesion promoter;
[0009] The inner coating layer comprises, by weight percentage, 10-15% of acrylate emulsion, 3-5% of PVDC emulsion, 0.3-0.5% of blending agent, 1-3% of ethyl acetoacetate methacrylate, 1-3% of polyethylene wax, 0.3-0.5% of leveling agent, and the balance is solvent.
[0010] Further, preferably: the thickness of the outer coating layer is 0.5-1.0 μm, the thickness of the BOPP base layer is 20-40 μm; and the thickness of the inner coating layer is 0.5-1.0 μm.
[0011] Further, preferably: the antioxidant is antioxidant 1010; the compatibilizer is PE-g-MAH; and the lubricant is erucamide or oleamide.
[0012] Furthermore, preferably, the conditioning agent is polyether-modified heptamethyltrisiloxane.
[0013] Furthermore, preferably, the solvent is a mixture of deionized water and an alcohol solvent in a ratio of 1:2-3.
[0014] Furthermore, preferably, the alcohol solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol, or a mixture of several of them.
[0015] Furthermore, preferably, the leveling agent is BYK-161 or BYK-331.
[0016] The present invention also provides a method for preparing a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film, comprising the following steps:
[0017] (1) Preparation of BOPP base layer: The BOPP raw material is mixed, extruded, stretched and corona treated to obtain a BOPP base layer film;
[0018] (2) respectively mixing the raw materials of the inner coating layer and the outer coating layer to form an inner coating liquid and an outer coating liquid for standby use;
[0019] (3) The mixed inner coating liquid and outer coating liquid are uniformly applied to the inner surface and outer surface of the BOPP base film respectively;
[0020] (4) The coated BOPP film is dried to evaporate the solvent, and finally a uniform upper coating layer and a lower coating layer are formed on the upper and lower surfaces of the BOPP film, respectively, to obtain a wrinkle-resistant cigarette packaging film.
[0021] Further, preferably: the preparation of the BOPP base layer comprises the following steps:
[0022] (1) according to the raw material ratio, the raw materials are mixed in a high-speed mixer for 20 minutes, extruded through a twin-screw granulator at an extrusion temperature of 230-240° C., extruded into a film, attached to a chilled roller with a high-pressure air knife to form a casting, and cooled and shaped by circulating cooling water;
[0023] (2) The cast sheet is drawn into BOPP film through a longitudinal stretching machine and a transverse stretching machine;
[0024] (3) The stretched BOPP film is subjected to corona treatment to obtain a BOPP base film.
[0025] Further, preferably: the drying process is 80-90°C for 1-2h.
[0026] Beneficial effects of the present invention:
[0027] The outer coating of the present invention is a composite of acrylate emulsion, multi-polymer emulsion and polyvinyl alcohol, which has the effect of improving the light aging resistance and wear resistance of BOPP film. The acrylic acid group in the acrylate emulsion can absorb ultraviolet rays, thereby reducing the intake of light energy and preventing or delaying the aging of the film; the multi-polymer emulsion not only enhances the chemical resistance of the coating, but also improves the resistance to light stability; the alcohol group in polyvinyl alcohol can increase the flexibility of the coating, reduce the generation of cracks, and improve the durability of the coating under repeated stress. The combination of acrylate and multi-polymer emulsion can provide more comprehensive ultraviolet absorption and barrier effects, while polyvinyl alcohol can improve the stability of the coating under high temperature and high humidity conditions.
[0028] Acrylic acid has relatively good hardness and wear resistance, which can improve the scratch resistance of the film surface. Multi-polymer emulsion provides better adhesion, making the coating and BOPP film more closely bonded, thereby improving the wear resistance of the overall coating; polyvinyl alcohol helps to improve the water dispersibility of the coating, which is particularly important in the production and processing of BOPP film, and can reduce the adverse effects of moisture on film performance. The introduction of multi-polymer emulsion increases the cross-linking density of the coating, while the flexibility of polyvinyl alcohol can reduce coating damage during friction. The combination of the three emulsions can significantly improve the adhesion between the coating and the BOPP film.
[0029] The inner coating of the present invention uses acrylic emulsion, PVDC emulsion, polyether-modified heptamethyltrisiloxane and acetoacetoxyethyl methacrylate, which have a mutually promoting effect in improving the barrier properties of the biaxially oriented polypropylene (BOPP) film:
[0030] Acrylate emulsion has good film-forming properties and water resistance. When added to BOPP film, it can increase the surface smoothness of the film, thereby improving its barrier properties. When it is used in combination with other modifiers such as PVDC emulsion, it can improve the mechanical properties of the film and make the barrier effect more durable. PVDC emulsion has excellent barrier properties and can significantly reduce the permeability of gases such as oxygen and water vapor. When used in combination with acrylate emulsion or polyether-modified heptamethyl trisiloxane, it can further improve the barrier properties of BOPP film while maintaining good flexibility and mechanical strength. Polyether-modified heptamethyl trisiloxane has excellent hydrophobicity and low surface tension, which can improve the waterproof properties of BOPP film. It can be used in combination with PVDC emulsion or acrylate emulsion to further improve the barrier properties of the film while improving processing performance and heat sealing properties. Acetoacetoxyethyl methacrylate has excellent barrier properties and can effectively reduce the permeability of gases such as oxygen and water vapor. When used together with the above-mentioned other modifiers, the barrier properties of BOPP film can be synergistically improved while maintaining good transparency and mechanical strength. Acrylate emulsion, PVDC emulsion, polyether-modified heptamethyltrisiloxane and acetoacetoxyethyl methacrylate can improve the barrier properties of BOPP film by forming a dense, uniform, and highly adhesive coating through their respective characteristics and interactions, effectively improving the barrier properties of the film.
[0031] The BOPP cigarette film of the present invention effectively solves the problems of the existing BOPP film by setting the inner and outer coatings, has excellent low-temperature heat sealing performance, will not stick to small packages, has good transparency and high gloss; has good moisture-proof barrier properties and strong aroma preservation; has good printability and clear inkjet coding; has strong wear resistance and can prevent scratches generated during packaging and transportation. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Acrylic emulsion uses water-based polyurethane acrylate, model: 177-E9002; multi-polymer emulsion uses Han ki nsMT5092A and polyvinyl alcohol use PVOA2488, and leveling agent uses BYK dispersant BYK-161; propylene-butane copolymer polypropylene F5005B is from Sinopec Beijing Yanshan Branch; metallocene polypropylene uses MPP6006 from PetroChina, and ethylene-propylene-butadiene terpolymer uses 5C30F from Basel; antioxidant is antioxidant 1010; compatibilizer is POE-g-MAH, from DuPont, USA, brand 22E703; lubricant is oleamide; adhesion promoter is bisaminosilane, using N-(2-aminoethyl)-3-aminopropyltrimethoxysilane with model KH792; PVDC emulsion uses P530 from Solvay, USA; blending agent is polyether-modified heptamethyltrisiloxane; and other raw materials are commercially available.
[0034] Example 1
[0035] A BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film, comprising an outer coating layer, a BOPP base layer and an inner coating layer;
[0036] The material of the outer coating layer includes, by weight percentage, 10% acrylic emulsion, 3% multi-polymer emulsion, 1% polyvinyl alcohol, 0.3% leveling agent, and the balance is solvent;
[0037] The material of the BOPP base layer includes, by weight percentage, 80% of propylene-butadiene copolymerized polypropylene, 10% of metallocene polypropylene, 4.7% of ethylene-propylene-butadiene terpolymer, 0.5% of antioxidant, 2% of compatibilizer, 0.5% of lubricant, and 2.3% of adhesion promoter;
[0038] The inner coating layer comprises, by weight percentage, 10% of acrylate emulsion, 3% of PVDC emulsion, 0.3% of blending agent, 1% of ethyl acetoacetate methacrylate, 1% of polyethylene wax, 0.3% of leveling agent, and the balance is solvent.
[0039] The solvent is a mixture of deionized water and an alcohol solvent in a ratio of 1:2. The alcohol solvent is ethanol.
[0040] The preparation method thereof comprises the following steps:
[0041] (1) Preparation of BOPP base layer: BOPP raw materials are mixed, extruded, stretched and corona treated to obtain BOPP base film, and the specific steps are as follows: 1) according to the raw material ratio, the raw materials are mixed in a high-speed mixer for 20 minutes, and extruded through a twin-screw granulator at an extrusion temperature of 230-240° C. to form a film, and the film is attached to a chilled roller with a high-pressure air knife to form a cast sheet, and then cooled and shaped by circulating cooling water;
[0042] 2) The cast sheet is drawn into a film through a longitudinal drawing machine and a transverse stretching machine; the sheet is preheated at 110°C, and then the sheet is longitudinally stretched at a certain speed, the stretching temperature is 70°C, the setting temperature is 100°C, and the stretching ratio is 5.5%; the longitudinally stretched sheet is preheated at 175°C, and then transversely stretched in a stretching zone with a certain expansion angle through a set chain guide rail to orient the polymer molecules in the transverse direction, the stretching temperature is 153°C, the setting temperature is 125°C, the stretching ratio is 700%, and air cooling is performed after setting;
[0043] 3) The stretched BOPP film is subjected to corona treatment to obtain a BOPP base film; the parameters during the corona treatment are as follows: the treatment voltage range is 15000V, the gap between the electrode and the film is controlled to be 2 mm, the output power range is 60kW, and the frequency adjustment range is 16kHz. Environmental requirements during corona treatment: humidity 50-65%, temperature at 35°C, and the corona machine works in an environment with an oxygen content of 45-55%.
[0044] (2) The raw materials of the inner coating layer and the outer coating layer are stirred in the liquid supply tank for a period of time to prepare coating liquids that can be used for coating. The prepared coating liquids are pumped into the intermediate material tanks through the liquid supply pump, and the inner coating liquid and the outer coating liquid are kept ready for use;
[0045] (3) The mixed inner coating liquid and outer coating liquid are uniformly coated on the inner surface and outer surface of the BOPP base film respectively, as follows: the intermediate pump pumps the coating liquid in the intermediate material tank into the closed scraper cavity, and the concave roller transfers the coating liquid in the cavity to the film surface through the contact angle with the film. The coating liquid is brought into the groove of the coating roller through the scraper cavity, and then transferred to the film through the coating roller to form a coating layer on the film surface. During the coating process, the running direction of the coating roller needs to be set to be opposite to the forward direction of the film to achieve the purpose of transferring the coating liquid. The present invention uses a coating system with double-sided coating, which requires two upper and lower coating rollers.
[0046] (4) The coated BOPP film is dried to volatilize the solvent, and finally a uniform upper coating layer and a lower coating layer are formed on the upper and lower surfaces of the BOPP film, respectively. The drying process is performed at 90° C. for 1 hour. Thus, an anti-wrinkle cigarette packaging film is obtained.
[0047] The thickness of the outer coating layer is 0.5 μm, the thickness of the BOPP base layer is 32 μm; and the thickness of the inner coating layer is 1.0 μm.
[0048] Example 2
[0049] The preparation method is the same as that of Example 1, except that: a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film comprises an outer coating layer, a BOPP base layer and an inner coating layer;
[0050] The material of the outer coating layer includes, by weight percentage, 13% acrylic emulsion, 4% multi-polymer emulsion, 1.6% polyvinyl alcohol, 0.4% leveling agent, and the balance is solvent;
[0051] The material of the BOPP base layer includes, by weight percentage, 75% of propylene-butadiene copolymerized polypropylene, 15% of metallocene polypropylene, 3% of ethylene-propylene-butadiene terpolymer, 1% of antioxidant, 3% of compatibilizer, 1% of lubricant, and 2% of adhesion promoter;
[0052] The inner coating layer comprises, by weight percentage, 13% of acrylate emulsion, 4% of PVDC emulsion, 0.4% of blending agent, 2% of ethyl acetoacetate methacrylate, 2% of polyethylene wax, 0.5% of leveling agent, and the balance is solvent.
[0053] Example 3
[0054] The preparation method is the same as that of Example 1, except that: a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film comprises an outer coating layer, a BOPP base layer and an inner coating layer;
[0055] The material of the outer coating layer includes, by weight percentage, 15% acrylic emulsion, 5% multi-polymer emulsion, 1.5% polyvinyl alcohol, 0.5% leveling agent, and the balance is solvent;
[0056] The material of the BOPP base layer includes, by weight percentage, 78% of propylene-butadiene copolymerized polypropylene, 13% of metallocene polypropylene, 3% of ethylene-propylene-butadiene terpolymer, 0.6% of antioxidant, 2.5% of compatibilizer, 0.6% of lubricant, and 2.3% of adhesion promoter;
[0057] The inner coating layer comprises, by weight percentage, 15% of acrylate emulsion, 5% of PVDC emulsion, 0.5% of blending agent, 3% of ethyl acetoacetate methacrylate, 3% of polyethylene wax, 0.4% of leveling agent, and the balance is solvent.
[0058] Example 4
[0059] The preparation method is the same as that of Example 1, except that: a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film comprises an outer coating layer, a BOPP base layer and an inner coating layer;
[0060] The material of the outer coating layer includes, by weight percentage, 12% acrylic emulsion, 4% multi-polymer emulsion, 2% polyvinyl alcohol, 0.5% leveling agent, and the balance is solvent;
[0061] The material of the BOPP base layer includes, by weight percentage, 78% of propylene-butadiene copolymerized polypropylene, 10% of metallocene polypropylene, 5% of ethylene-propylene-butadiene terpolymer, 1% of antioxidant, 3% of compatibilizer, 1% of lubricant, and 2% of adhesion promoter;
[0062] The inner coating layer comprises, by weight percentage, 12% of acrylate emulsion, 5% of PVDC emulsion, 0.5% of blending agent, 2% of ethyl acetoacetate methacrylate, 2% of polyethylene wax, 0.5% of leveling agent, and the balance is solvent.
[0063] Example 5
[0064] The preparation method is the same as that of Example 1, except that: a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film comprises an outer coating layer, a BOPP base layer and an inner coating layer;
[0065] The material of the outer coating layer includes, by weight percentage, 14% acrylic emulsion, 3% multi-polymer emulsion, 1.8% polyvinyl alcohol, 0.4% leveling agent, and the balance is solvent;
[0066] The material of the BOPP base layer includes, by weight percentage, 76% of propylene-butadiene copolymerized polypropylene, 14% of metallocene polypropylene, 4% of ethylene-propylene-butadiene terpolymer, 0.7% of antioxidant, 2.5% of compatibilizer, 0.7% of lubricant, and 2.1% of adhesion promoter;
[0067] The inner coating layer comprises, by weight percentage, 14% of acrylate emulsion, 4% of PVDC emulsion, 0.4% of blending agent, 2.5% of ethyl acetoacetate methacrylate, 2.5% of polyethylene wax, 0.3% of leveling agent, and the balance is solvent.
[0068] The properties of the BOPP films prepared in Examples 1-5 were measured, and the specific results are shown in Table 1.
[0069] Initial heat seal temperature detection: During the test, the initial heat seal temperature is set to 110°C, the sample is folded in half, the two ends are aligned and placed flat on the welding surface of the heat sealer for heat sealing. The welding surface pressure during heat sealing is 0.18MPa, and the heat sealing time is 0.5S. After the sealed sample has cooled, gently pull the heat seal by hand. If the heat seal is intact, adjust the heat seal setting temperature down by 1 degree until the critical temperature for sealing is found. If the heat seal is not good and the sample is separated, adjust the heat seal temperature upward. Heat seal the sample at the critical temperature. After the sealed sample has cooled, gently pull the heat seal by hand. If 2 / 3 of the heat seal is torn, confirm that this temperature is the initial heat seal temperature.
[0070] Table 1 BOPP film performance test results prepared in different embodiments
[0071]
[0072] As can be seen from Table 1, the BOPP cigarette film of the present invention effectively solves the problems of the existing BOPP film by setting the inner and outer coatings, has excellent low-temperature heat sealing performance, will not stick to small packages, has good transparency and high gloss; has good moisture barrier properties and strong aroma retention; has good printability and clear inkjet coding; has strong wear resistance and can prevent scratches generated during packaging and transportation.
[0073] Examples 6-10 investigate the effects of different coating thicknesses on BOPP cigarette film
[0074] The raw materials and preparation method are the same as those in Example 1, except for the coating thickness, as shown in Table 2.
[0075] Table 2 BOPP film performance test results prepared in different embodiments
[0076]
[0077]
[0078] It can be seen from Table 2 that coatings of different thicknesses have an important influence on the haze, gloss, hot air intensity, sealing temperature, moisture permeability and friction coefficient of BOPP cigarette film.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film, characterized in that: Including outer coating layer, BOPP base layer and inner coating layer; The material of the outer coating layer includes, by weight percentage, 10-15% acrylic emulsion, 3-5% multi-polymer emulsion, 1-2% polyvinyl alcohol, 0.3-0.5% leveling agent, and the balance is solvent; The material of the BOPP base layer includes, by weight percentage, 75-80% of propylene-butadiene copolymerized polypropylene, 10-15% of metallocene polypropylene, 3-5% of ethylene-propylene-butadiene terpolymer, 0.5-1% of antioxidant, 2-3% of compatibilizer, 0.5-1% of lubricant, and 2-2.3% of adhesion promoter; The inner coating layer comprises, by weight percentage, 10-15% of acrylate emulsion, 3-5% of PVDC emulsion, 0.3-0.5% of blending agent, 1-3% of ethyl acetoacetate methacrylate, 1-3% of polyethylene wax, 0.3-0.5% of leveling agent, and the balance is solvent.
2. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 1, characterized in that: The thickness of the outer coating layer is 0.5-1.0 μm, the thickness of the BOPP base layer is 20-40 μm; the thickness of the inner coating layer is 0.5-1.0 μm.
3. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 1, characterized in that: Preferably: the antioxidant is antioxidant 1010; the compatibilizer is PE-g-MAH; and the lubricant is erucamide or oleamide.
4. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 1, characterized in that: The conditioning agent is polyether-modified heptamethyltrisiloxane.
5. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 1, characterized in that: The solvent is a mixture of deionized water and an alcohol solvent in a ratio of 1:2-3.
6. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 5, characterized in that: The alcohol solvent is one of methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol, or a mixture of the two or more thereof.
7. The BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film according to claim 1, characterized in that: The leveling agent is BYK-161 or BYK-331; the adhesion promoter is bisaminosilane.
8. A method for preparing a BOPP water-based acrylic acid coated wrinkle-resistant cigarette packaging film as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Preparation of BOPP base layer: The BOPP raw material is mixed, extruded, stretched and corona treated to obtain a BOPP base layer film; (2) respectively mixing the raw materials of the inner coating layer and the outer coating layer to form an inner coating liquid and an outer coating liquid for standby use; (3) The mixed inner coating liquid and outer coating liquid are uniformly applied to the inner surface and outer surface of the BOPP base film respectively; (4) The coated BOPP film is dried to evaporate the solvent, and finally a uniform upper coating layer and a lower coating layer are formed on the upper and lower surfaces of the BOPP film, respectively, to obtain a wrinkle-resistant cigarette packaging film.
9. The preparation method according to claim 8, characterized in that: The preparation of the BOPP base layer comprises the following steps: (1) according to the raw material ratio, the raw materials are mixed in a high-speed mixer for 20 minutes, extruded through a twin-screw granulator at an extrusion temperature of 230-240° C., extruded into a film, attached to a chilled roller with a high-pressure air knife to form a casting, and cooled and shaped by circulating cooling water; (2) The cast sheet is drawn into BOPP film through a longitudinal stretching machine and a transverse stretching machine; (3) The stretched BOPP film is subjected to corona treatment to obtain a BOPP base film.
10. The preparation method according to claim 8, characterized in that: The drying process is 80-90° C., 1-2 h.