High-performance shock-absorbing noise-reducing low-emission long glass fiber reinforced polypropylene composite material and preparation method thereof

By adjusting the component ratio and treatment method of long glass fiber reinforced polypropylene composite materials, the problems of difficulty in processing, high cost and recycling are solved, and high-performance and low-cost composite materials are achieved, which improves the toughness and mechanical properties of the material. Suitable for automobiles and other fields.

CN118956057APending Publication Date: 2024-11-15JURONG BASTEP COMPOSITE MATERIALS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411143987.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional long glass fiber reinforced polypropylene composites have challenges in terms of difficult processing, high cost and recycling, which limits their wide application in automobiles and other fields.

Method used

By adjusting the component ratio, adding materials such as polyurethane, wood pulp fiber, butyl rubber, talc powder and titanium dioxide, combined with ultrasonic dispersion and even stirring, a low-cost, recyclable high-performance composite material is prepared.

Benefits of technology

It improves the toughness, wear resistance and mechanical properties of the material, reduces fluidity, enhances adhesive performance and cost-effectiveness, and meets the performance needs of automobiles and other fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-performance shock-absorbing noise-reducing low-emission long glass fiber reinforced polypropylene composite material and a preparation method thereof, and belongs to the field of preparation of composite materials, the composite material is prepared from the following components by mass: 60-80 parts of polypropylene; 8 to 12 parts of long glass fiber; 6 to 8 parts of polyurethane; 5 to 9 parts of wood pulp fiber; 5-9 parts of butadiene rubber; 6-8 parts of talcum powder; 2 to 4 parts of titanium dioxide; 6-8 parts of a light stabilizer; and 3-7 parts of a compatilizer. The polyurethane material is adopted, the polyurethane material has excellent wear resistance, oil resistance and aging resistance, when the polyurethane material is used for manufacturing some automobile damping parts, compared with some high-end damping materials, the cost of the polyurethane material is relatively low, and meanwhile certain damping requirements can be met. The polypropylene composite material which is low in raw material cost, can be recycled and is simple and convenient to process is prepared through combination of multiple added components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of composite materials, in particular to a high-performance shock-absorbing, noise-reducing and low-emission long glass fiber reinforced polypropylene composite material and a preparation method thereof. Background Art

[0002] With the rapid development of the automobile industry, the requirements for automobile materials are also increasing. Traditional metal materials have many limitations in terms of shock absorption, noise reduction, low emission and lightweight. In addition, due to the popularity of trams, functional high-quality materials have become a research hotspot, and the development of new high-performance composite materials has become one of the difficult problems that technicians in this field need to overcome. Long glass fiber reinforced polypropylene composite materials have gradually been widely used in the fields of automobiles, transportation, construction, and chemicals due to their excellent mechanical properties, formability, corrosion resistance, and recyclability.

[0003] Long glass fiber reinforced polypropylene composite material is based on thermoplastic resin polypropylene and long glass fiber as a reinforcing skeleton. It has the characteristics of low density, high strength, good impact resistance, high specific modulus, etc. The above advantages make it a sought-after material in the automotive field.

[0004] However, there are still some technical defects in its actual application, including: difficult processing: long glass fibers are prone to breakage and uneven distribution during the injection molding process, resulting in reduced product performance; high cost: compared with traditional materials, the production cost of composite materials is higher, which to a certain extent limits its application in large-scale production. Cannot be recycled and reused: the separation problem of fiber and resin needs to be solved during the recycling process of composite materials. The above defects limit the production and use of polypropylene composite materials. Summary of the invention

[0005] The present invention aims at the defects existing in the prior art, and prepares a polypropylene composite material which has low raw material cost, can be recycled and is easy to process by adding a combination of multiple components.

[0006] The present invention is achieved in that:

[0007] A high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material, characterized in that, in parts by mass, the composite material is prepared from the following components:

[0008] Polypropylene: 60-80 parts;

[0009] Long glass fiber: 8-12 parts;

[0010] Polyurethane: 6-8 parts;

[0011] Wood pulp fiber: 5-9 parts;

[0012] Butadiene rubber: 5-9 parts;

[0013] Talc: 6-8 parts;

[0014] Titanium dioxide: 2-4 parts;

[0015] Light stabilizer: 6-8 parts;

[0016] Compatibilizer: 3 to 7 parts.

[0017] Furthermore, the light stabilizer is salicylate.

[0018] Furthermore, the compatibilizer is polypropylene grafted maleic anhydride polymer.

[0019] Furthermore, the particle size of the titanium dioxide is 5 to 20 nanometers.

[0020] Furthermore, the particle size of the talcum powder is 30 to 50 microns.

[0021] Furthermore, the mass ratio of the polypropylene to the polyurethane is 10:1.

[0022] Furthermore, the mass ratio of the wood pulp fiber to the butadiene rubber is 1:1.

[0023] Furthermore, the composite material is prepared from the following components in parts by mass:

[0024] Polypropylene: 70 parts;

[0025] Long glass fiber: 10 parts;

[0026] Polyurethane: 7 parts;

[0027] Wood pulp fiber: 8 parts;

[0028] Butadiene rubber: 8 parts;

[0029] Talc: 7 parts;

[0030] Titanium dioxide: 3 parts;

[0031] Light stabilizer: 8 parts;

[0032] Compatibilizer: 6 parts.

[0033] A method for preparing a high-performance shock-absorbing, noise-reducing, and low-emission long glass fiber reinforced polypropylene composite material, characterized in that the method comprises:

[0034] Step 1, weighing 5 to 9 parts of wood pulp fiber, 5 to 9 parts of butadiene rubber, 6 to 8 parts of talc, and 2 to 4 parts of titanium dioxide according to mass parts, ultrasonically dispersing the above materials at 50±5°C for 30 minutes, and then stirring them evenly for use;

[0035] Step 2: Add 60-80 parts of polypropylene, 8-12 parts of long glass fibers, 6-8 parts of polyurethane, and 3-7 parts of compatibilizer to the mixture of step 1, and mix the above substances for reaction at a reaction temperature of 200±20°C for 30 minutes until the mixture is uniformly mixed.

[0036] Step 3: Add 6 to 8 parts of light stabilizer into the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min. After mixing, extrude and granulate.

[0037] The beneficial effects of the present invention compared with the prior art are:

[0038] The present invention adopts polyurethane material, which has excellent wear resistance, oil resistance and aging resistance. When used to manufacture some automotive shock-absorbing components, the cost of polyurethane material is relatively low compared with some high-end shock-absorbing materials, and at the same time it can meet certain shock-absorbing requirements. In addition, the adhesion can be enhanced: although it is difficult to directly bond polypropylene and polyurethane, the adhesion performance of polypropylene and other materials can be significantly improved by adding a compatibilizer to graft maleic anhydride polymer to polypropylene. Polyurethane has good wear resistance, aging resistance and thermal stability, which helps to improve the overall performance of composite materials. Improve toughness: The addition of polyurethane can increase the toughness of polypropylene composite materials, reduce the occurrence of brittle fracture, and improve the impact resistance of the material.

[0039] In the present invention, the dimensional stability is improved by adding wood pulp fibers: the addition of wood pulp fibers can improve the dimensional stability of the polypropylene composite material and reduce the dimensional changes caused by temperature changes or humidity changes. In addition, the cost can be reduced: as a natural renewable resource, the cost of wood pulp fibers is relatively low, which helps to reduce the overall cost of the polypropylene composite material.

[0040] In the present invention, the fluidity is reduced by adding cis-1,4-dimethoxy-1-butadiene rubber: the addition of cis-1,4-dimethoxy-1-butadiene rubber can reduce the fluidity of the polypropylene composite material, which helps to control the flow behavior of the material during processing and improve the molding accuracy of the product. Improve wear resistance: cis-1,4-dimethoxy-1-butadiene rubber has excellent wear resistance, which can improve the wear resistance of the polypropylene composite material and extend the service life of the material.

[0041] The combination of talcum powder and titanium dioxide in the present invention can increase the strength and hardness of the polypropylene matrix and improve the mechanical properties of the composite material. Furthermore, talcum powder, as a cheap inorganic filler, can significantly reduce the raw material cost of the polypropylene composite material. The combination of multiple components in the present invention can jointly improve the performance of the composite material in the polypropylene composite material, meeting the requirements for material performance in automobiles and even more other fields. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail by enumerating examples below. It should be noted that the specific implementation described here is only used to explain the present invention and is not used to limit the present invention.

[0043] Example 1

[0044] In this embodiment, a preparation method of a high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material is as follows:

[0045] Step 1. Weigh 6 parts of wood pulp fiber, 6 parts of butyl rubber, 7 parts of talcum powder, and 3 parts of titanium dioxide according to mass parts, ultrasonically disperse the above materials at 50±5°C for 30 minutes, and then stir them evenly for use; the mass ratio of the wood pulp fiber to the butyl rubber is 1:1.

[0046] Step 2: Add 75 parts of polypropylene, 10 parts of long glass fiber, 7.5 parts of polyurethane and 5 parts of compatibilizer to the mixture of step 1, and mix the above substances for reaction. The reaction parameters are: 200±20℃, time: 30min, and mix evenly. The mass ratio of the polypropylene to the polyurethane is 10:1. The compatibilizer is polypropylene grafted maleic anhydride polymer.

[0047] Step 3: Add 7 parts of light stabilizer to the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min, and after mixing, extrude and granulate. The light stabilizer is salicylic acid.

[0048] Example 2

[0049] In this embodiment, a preparation method of a high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material is as follows:

[0050] Step 1, weigh according to mass: 5 parts of wood pulp fiber, 5 parts of butadiene rubber, 6 parts of talcum powder, and 2 parts of titanium dioxide, ultrasonically disperse the above materials at 50±5°C for 30 minutes, and then stir them evenly for use; the mass ratio of the wood pulp fiber to the butadiene rubber is 1:1.

[0051] Step 2: Add 60 parts of polypropylene, 8 parts of long glass fiber, 6 parts of polyurethane and 3 parts of compatibilizer to the mixture in step 1, mix and react the above substances, the reaction parameters are: 200±20℃, time: 30min, mix evenly; the mass ratio of the polypropylene to the polyurethane is 10:1. The compatibilizer is polypropylene grafted maleic anhydride polymer.

[0052] Step 3: Add 6 parts of light stabilizer to the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min, and extrude and granulate after mixing. The light stabilizer is salicylic acid.

[0053] Example 3

[0054] In this embodiment, a preparation method of a high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material is as follows:

[0055] Step 1, weigh 9 parts of wood pulp fiber, 9 parts of butadiene rubber, 8 parts of talcum powder, and 4 parts of titanium dioxide according to mass parts, ultrasonically disperse the above materials at 50±5°C for 30 minutes, and then stir them evenly for use; the mass ratio of the wood pulp fiber to the butadiene rubber is 1:1.

[0056] Step 2: Add 80 parts of polypropylene, 12 parts of long glass fiber, 8 parts of polyurethane and 7 parts of compatibilizer to the mixture of step 1, mix and react the above substances, the reaction parameters are: 200±20℃, time: 30min, mix evenly; the mass ratio of the polypropylene to the polyurethane is 10:1. The compatibilizer is polypropylene grafted maleic anhydride polymer.

[0057] Step 3: Add 8 parts of light stabilizer to the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min, and after mixing, extrude and granulate. The light stabilizer is salicylic acid.

[0058] Example 4

[0059] In this embodiment, a preparation method of a high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material is as follows:

[0060] Step 1, weigh according to mass: 7 parts of wood pulp fiber, 7 parts of butadiene rubber, 6 parts of talcum powder, 2-4 parts of titanium dioxide, ultrasonically disperse the above materials at 50±5°C for 30 minutes, and then stir them evenly for use; the mass ratio of the wood pulp fiber to the butadiene rubber is 1:1.

[0061] Step 2: Add 65 parts of polypropylene, 9 parts of long glass fiber, 6.5 parts of polyurethane and 4 parts of compatibilizer to the mixture of step 1, and mix the above substances for reaction. The reaction parameters are: 200±20℃, time: 30min, and mix evenly. The mass ratio of the polypropylene to the polyurethane is 10:1. The compatibilizer is polypropylene grafted maleic anhydride polymer.

[0062] Step 3: Add 6-8 parts of light stabilizer to the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min, and extrude and granulate after mixing. The light stabilizer is salicylic acid.

[0063] Example 5

[0064] In this embodiment, a preparation method of a high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material is as follows:

[0065] Step 1, weigh according to mass: 8 parts of wood pulp fiber, 8 parts of butadiene rubber, 7 parts of talc powder, and 3 parts of titanium dioxide, ultrasonically disperse the above materials at 50±5°C for 30 minutes, and then stir them evenly for use; the mass ratio of the wood pulp fiber to the butadiene rubber is 1:1.

[0066] Step 2: Add 70 parts of polypropylene, 10 parts of long glass fiber, 7 parts of polyurethane and 6 parts of compatibilizer to the mixture of step 1, mix and react the above substances, the reaction parameters are: 200±20℃, time: 30min, mix evenly; the mass ratio of the polypropylene to the polyurethane is 10:1. The compatibilizer is polypropylene grafted maleic anhydride polymer.

[0067] Step 3: Add 8 parts of light stabilizer to the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min, and after mixing, extrude and granulate. The light stabilizer is salicylic acid.

[0068] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.

Claims

1. A high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material, characterized in that: The composite material is prepared from the following components in parts by mass: Polypropylene: 60-80 parts; Long glass fiber: 8-12 parts; Polyurethane: 6-8 parts; Wood pulp fiber: 5-9 parts; Butadiene rubber: 5-9 parts; Talc: 6-8 parts; Titanium dioxide: 2-4 parts; Light stabilizer: 6-8 parts; Compatibilizer: 3 to 7 parts.

2. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The light stabilizer is salicylic acid.

3. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The compatibilizer is polypropylene grafted maleic anhydride polymer.

4. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The particle size of the titanium dioxide is 5 to 20 nanometers.

5. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The particle size of the talcum powder is 30 to 50 microns.

6. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The mass ratio of the polypropylene to the polyurethane is 10:

1.

7. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The mass ratio of the wood pulp fiber to the butadiene rubber is 1:

1.

8. The high-performance shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The composite material is prepared from the following components in parts by mass: Polypropylene: 70 parts; Long glass fiber: 10 parts; Polyurethane: 7 parts; Wood pulp fiber: 8 parts; Butadiene rubber: 8 parts; Talc: 7 parts; Titanium dioxide: 3 parts; Light stabilizer: 8 parts; Compatibilizer: 6 parts.

9. The method for preparing a high-performance vibration-absorbing, noise-reducing and low-emission long glass fiber reinforced polypropylene composite material according to any one of claims 1 to 8, characterized in that: The method described is: Step 1, weighing 5 to 9 parts of wood pulp fiber, 5 to 9 parts of butadiene rubber, 6 to 8 parts of talc, and 2 to 4 parts of titanium dioxide according to mass parts, ultrasonically dispersing the above materials at 50±5°C for 30 minutes, and then stirring them evenly for use; Step 2: Add 60-80 parts of polypropylene, 8-12 parts of long glass fibers, 6-8 parts of polyurethane and 3-7 parts of compatibilizer are mixed and reacted at 200±20℃ for 30min until mixed evenly. Step 3: Add 6 to 8 parts of light stabilizer into the mixed material extruder, and continue mixing. The mixing parameters are: 300±20℃, time: 30min. After mixing, extrude and granulate.

Citation Information

Cited By

  • Shock-absorbing, noise-reducing and low-emission long glass fiber reinforced polypropylene composite material with good surface appearance for automotive trim and preparation method thereof

    CN117186541A

  • Shock-absorbing, noise-reducing, low-emission long glass fiber reinforced polypropylene composite material with good surface appearance for automobile interior and preparation method thereof

    CN117186541B