IBC battery

By using high-hard silicone insulating glue in IBC batteries, combining glass fibers and modified inorganic fillers, the short circuit problem caused by insufficient hardness of the silicone insulating glue is solved, and the reliability and application range of the battery are improved.

CN118956264APending Publication Date: 2024-11-15JA SOLAR TECH YANGZHOU

Patent Information

Application Number
CN202410898739.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The low hardness of silicone insulating glue in IBC batteries leads to easy short circuit during welding and lamination, which limits its application.

Method used

Using high-hardness silicone insulating glue, the hardness and bond strength of the insulating glue are improved by adding glass fibers to polyalkyl vinyl siloxane and cross-linking reaction, combining modified inorganic fillers and specific additives.

Benefits of technology

It effectively avoids short circuits caused by changes in insulating glue thickness during welding and lamination, improves the reliability of components, and expands the application potential of silicone insulating glue in the field of IBC batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956264A_ABST
    Figure CN118956264A_ABST
Patent Text Reader

Abstract

The invention relates to an IBC battery, and belongs to the technical field of solar batteries. The IBC battery comprises a positive pole main grid line, a positive pole fine auxiliary grid line, a negative pole main grid line and a negative pole fine auxiliary grid line which are distributed on the back face of the IBC battery, and the tail end of the positive pole fine auxiliary grid line and the tail end of the negative pole fine auxiliary grid line are both coated with high-hardness organic silicon insulation glue. The high-hardness organic silicon insulating glue comprises polyalkyl vinyl siloxane and glass fibers, and the mass ratio of the glass fibers to the polyalkyl vinyl siloxane is smaller than or equal to 1: 4. According to the invention, the glass fiber which can be subjected to a cross-linking reaction with the polyalkyl vinyl siloxane is added into the organic silicon insulation paste taking the polyalkyl vinyl siloxane as a main body, so that the cross-linking degree of the organic silicon insulation paste can be improved, and the hardness of the organic silicon insulation paste is further improved; the organic silicon insulation glue is used for carrying out insulation protection on the tail ends of the positive electrode fine auxiliary grid lines and the negative electrode fine auxiliary grid lines, so that short circuit caused by thickness change of the organic silicon insulation glue due to extrusion in the welding and laminating processes of the welding strip can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an IBC battery, belonging to the technical field of solar cells. Background Art

[0002] The main feature of the IBC (Interdigitated Back Contact) battery is that the positive and negative electrodes of the battery are distributed on the back of the battery, and the front of the battery is unobstructed. It has a high photoelectric conversion efficiency and has attracted much attention from the industry. It has become a research hotspot for the new generation of solar cell technology. Among them, the positive and negative electrodes of the IBC battery both contain main grid lines and thin auxiliary grid lines. The fine grid lines of the positive and negative electrodes are arranged in a forked shape on the back of the battery. The main grid lines in the positive electrode are printed vertically with the auxiliary fine grid lines, and the main grid lines in the negative electrode are printed vertically with the auxiliary fine grid lines. In the subsequent welding process of the welding ribbon, the welding ribbon needs to be laid along the direction of the main grid lines in the IBC battery for welding, but when the welding ribbon is swayed and misplaced, it is very easy to overlap with the auxiliary fine grid lines of the opposite electrode and cause a short circuit. In order to prevent the positive and negative grid lines from being turned on and causing a short circuit, insulating glue is usually printed at the ends of the positive and negative auxiliary fine grid lines for insulation protection.

[0003] The insulating adhesive systems currently used in the industry mainly include epoxy resin systems, acrylate systems, silicone systems, etc. Compared with epoxy resin and acrylic resin system insulating adhesives, silicone system insulating adhesives have higher temperature resistance, low elastic modulus and good chemical stability. However, there are the following problems in the application of silicone insulating adhesives: As an elastomer, the hardness of silicone insulating adhesive is relatively small, especially in the process of welding and laminating the welding strips, the insulating adhesive is more susceptible to extrusion and thickness changes. The weakened insulation performance may even cause the grid line to be exposed and directly contact the welding strip, resulting in a short circuit, which in turn limits the application of silicone insulating adhesives in the field of IBC batteries. Summary of the invention

[0004] In view of the problem that the current IBC battery is prone to short circuit due to the low hardness of the silicone insulating glue, the present invention provides an IBC battery, in which high-hardness silicone insulating glue is used to insulate the ends of the secondary fine grid lines, and the silicone insulating glue uses polyalkyl vinyl siloxane as the silicone insulating glue matrix, and an appropriate amount of glass fiber is added to make it cross-linked with the silicone insulating glue matrix, so as to further improve the cross-linking degree of the silicone insulating glue matrix, and then improve the hardness of the silicone insulating glue, so as to avoid short circuit caused by thickness change of the silicone insulating glue due to extrusion during the welding and lamination process of the welding strip.

[0005] The objectives of the present invention are achieved through the following technical solutions.

[0006] An IBC battery comprises a positive main grid line, a positive fine sub-grid line, a negative main grid line and a negative fine sub-grid line distributed on the back of the IBC battery, wherein the positive main grid line is perpendicular to the positive fine sub-grid line, the negative main grid line is perpendicular to the negative fine sub-grid line, the positive sub-fine grid line and the negative sub-fine grid line are arranged in a forked finger shape, and the end of the positive sub-fine grid line does not contact the negative main grid line, and the end of the negative sub-fine grid line does not contact the positive main grid line, and the end of the positive sub-fine grid line and the end of the negative sub-fine grid line are both coated with high-hardness organic silicon insulating glue;

[0007] The high-hardness organic silicon insulating adhesive comprises components of polyalkyl vinyl siloxane and glass fiber, wherein the mass ratio of glass fiber to polyalkyl vinyl siloxane is less than or equal to 1:4, preferably 1:4 to 1:14.

[0008] Furthermore, the alkyl group in the polyalkylvinylsiloxane is an alkyl group having no more than 5 carbon atoms in the main chain.

[0009] Furthermore, the glass fiber has a diameter of 8 to 30 μm and a length of 3 to 20 mm.

[0010] Furthermore, the glass fiber is pretreated before use by the following method: first, the glass fiber is burned at 600-800°C for 20-30 minutes, then soaked in a 0.5-3% by mass silane coupling agent aqueous solution for 10-15 minutes, and finally baked at 100-120°C for 10-15 minutes. The above pretreatment is beneficial to improve the temperature resistance, purity and surface energy of the glass fiber, and improve the compatibility of the glass fiber with the silicone insulating adhesive matrix.

[0011] Furthermore, the components of the high-hardness organic silicone insulating adhesive also include modified inorganic fillers, wherein the mass ratio of the modified inorganic filler to the glass fiber is 1:3 to 3:1, and the modified inorganic filler is at least one of hydroxylated silica, calcium carbonate, alumina, magnesia and mica.

[0012] Furthermore, the particle size of the modified inorganic filler is 5 to 10 μm.

[0013] Furthermore, the modified inorganic filler is obtained by the following method: the inorganic filler, propylene oxide, boron trifluoride etherate and dichloromethane are mixed, reacted at -35 to -10°C for 4 to 6 hours under a protective atmosphere, then restored to room temperature, and then allowed to stand for 10 to 25 hours to obtain a hydroxylated modified inorganic filler.

[0014] Furthermore, the molar ratio of glycidol to boron trifluoride ether is 8:1-11:1, the concentration of glycidol in dichloromethane is 3-5 mol / L, and the concentration of the inorganic filler in dichloromethane is 2-3 g / mL.

[0015] Furthermore, the mass ratio of the polyalkyl vinyl siloxane to the sum of the glass fiber and the modified inorganic filler is 2:1 to 3.5:1.

[0016] Furthermore, the composition of the high-hardness organic silicon insulating adhesive also includes at least one of an adhesion promoter, a curing agent, a silane coupling agent, an active monomer and a dispersant;

[0017] The adhesion promoter is at least one of γ-aminopropyl triethoxysilane, γ-glycidyloxypropyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane, and the adhesion promoter can further improve the surface energy of the organic silicone insulating adhesive and enhance the bonding strength of the organic silicone insulating adhesive;

[0018] The curing agent is at least one of vinyltriamine, diethylenetriamine and dimethylaminopropylamine, and the curing agent is beneficial to promote the cross-linking reaction of polyalkyl vinyl siloxane;

[0019] The silane coupling agent can further improve the compatibility between the glass fiber and the organic silicon insulating adhesive;

[0020] The active monomer is at least one of polymethyl hydrogen siloxane, polyethyl hydrogen siloxane and polypropyl hydrogen siloxane, and the active monomer is used to adjust the viscosity of the organic silicon insulating adhesive;

[0021] The dispersant is at least one of polyvinyl alcohol, polyamide and polyvinyl acetate, and the dispersant is conducive to uniform dispersion of the modified inorganic filler in the organic silicon insulating adhesive to avoid agglomeration;

[0022] Among them, when the mass fraction of polyalkyl vinyl siloxane in the high hardness silicone insulating glue is 60 to 70 parts, the mass fraction of adhesion promoter is preferably 3 to 5 parts, the mass fraction of curing agent is preferably 1 to 3 parts, the mass fraction of silane coupling agent is preferably 0.1 to 1 part, the mass fraction of active monomer is preferably 4 to 8 parts, and the mass fraction of dispersant is preferably 1 to 5 parts.

[0023] Furthermore, the composition of a high-hardness silicone insulating adhesive and the mass fraction of each component are as follows: 60-70 parts of polyalkyl vinyl siloxane, 5-15 parts of glass fiber, 5-15 parts of modified inorganic filler, 3-5 parts of adhesion promoter, 1-3 parts of curing agent, 0.1-1 part of silane coupling agent, 4-8 parts of active monomer, and 1-5 parts of dispersant.

[0024] The preparation method of the high-hardness organic silicon insulating adhesive comprises the following steps: firstly, polyalkyl vinyl siloxane, glass fiber, modified inorganic filler, adhesion promoter, active monomer and dispersant are mixed evenly to obtain a primary mixture; then, a silane coupling agent is added and mixed evenly to obtain a secondary mixture; and finally, a curing agent is added and mixed evenly to obtain the organic silicon insulating adhesive.

[0025] Further, in the process of obtaining the preliminary mixture, the stirring temperature is 30-40°C, the stirring rate is 50-80 rpm, and the stirring time is 15-20 min;

[0026] In the process of adding the silane coupling agent to obtain the secondary mixture, the stirring temperature is 50-60° C., the stirring rate is 30-40 rpm, and the stirring time is 20-30 min;

[0027] In the process of adding the curing agent to obtain the organic silicon insulating adhesive, the stirring temperature is 50-60° C., the stirring speed is 30-40 rpm, and the stirring time is 20-30 min.

[0028] The IBC cell further includes a silicon substrate, an n+ diffusion layer disposed on the front side of the silicon substrate, a first passivation layer disposed on the n+ diffusion layer, a first anti-reflection layer disposed on the first passivation layer, a local n+ diffusion layer and a local p+ diffusion layer disposed on the back side of the silicon substrate, a second passivation layer disposed on the local n+ diffusion layer and the local p+ diffusion layer, a second anti-reflection layer disposed on the second passivation layer, and a positive electrode and a negative electrode disposed on the second anti-reflection layer, wherein the positive electrode is electrically connected to the local p+ diffusion layer, and the negative electrode is electrically connected to the local n+ diffusion layer;

[0029] The positive electrode includes the positive electrode main grid line and the positive electrode auxiliary fine grid line; the negative electrode includes the negative electrode main grid line and the negative electrode auxiliary fine grid line.

[0030] Beneficial effects:

[0031] (1) The present invention uses polyalkyl vinyl siloxane as the matrix of the organic silicone insulating adhesive and introduces glass fiber. On the one hand, the excellent toughening effect of the glass fiber itself is utilized. The addition of glass fiber can improve the hardness of the organic silicone insulating adhesive itself to a certain extent; on the other hand, a cross-linking reaction occurs between the glass fiber and the polyalkyl vinyl siloxane, thereby increasing the cross-linking degree of the organic silicone insulating adhesive matrix, and further increasing the hardness of the organic silicone insulating adhesive.

[0032] (2) The Si-O-Si bond energy formed after the organic silicon insulating adhesive is printed and cured is very large, which easily leads to very low bonding strength between the organic silicon insulating adhesive and the adhesive film during the lamination process. Once slippage occurs between the adhesive film and the organic silicon insulating adhesive, there is a hidden danger of air entering, thereby increasing the reliability risk of the component. The present invention adds modified inorganic fillers to the organic silicon insulating adhesive, and uses hydroxylated inorganic fillers to increase the surface energy of the organic silicon insulating adhesive, which can correspondingly form good chemical contact with the adhesive film. During the lamination process, the hydroxyl group reacts with the adhesive film to form a bond, thereby improving the bonding strength between the organic silicon insulating adhesive and the adhesive film. In addition, when blended with glass fiber, some of the large number of hydroxyl groups on the surface of the modified inorganic filler will undergo a migration effect and be dispersed on the surface of the glass fiber. When the modified inorganic filler, glass fiber and polyalkyl vinyl siloxane are mixed, the hydroxyl groups are dispersed more evenly on the surface of the silicone insulating adhesive, which is beneficial to further increase the surface tension of the silicone insulating adhesive, and its peeling force with the adhesive film is correspondingly increased; and because the particle size difference between the two is relatively large, agglomeration can be avoided, so that the modified inorganic filler is dispersed more evenly, which is beneficial to further improve the hardness of the silicone insulating adhesive.

[0033] (3) If the amount of glass fiber added is too little, the effect of improving the hardness of the silicone insulating adhesive is not good, and the effect of improving the uniform dispersion of hydroxyl groups in the modified inorganic filler in the silicone insulating adhesive is not good; however, excessive glass fiber will form steric hindrance, making the cross-linking reaction of polyalkyl vinyl siloxane difficult and affecting the degree of cross-linking. If the amount of modified inorganic filler added is too little, the effect of improving the bonding strength of the silicone insulating adhesive is not good, but if the amount is too much, the modified inorganic filler will easily agglomerate and phase separation will easily occur when it is mixed with polyalkyl vinyl siloxane. Therefore, by adjusting the amount of glass fiber and modified inorganic filler added, silicone insulating adhesives with different hardness and bonding strength can be obtained.

[0034] (4) Adding adhesion promoter, curing agent, silane coupling agent, active monomer and dispersant to the silicone insulating adhesive with polyalkyl vinyl siloxane as the main body is beneficial to further improve the hardness and bonding strength of the silicone insulating adhesive. It can be selectively added according to actual needs to meet the requirements of different application scenarios.

[0035] (5) The preparation method of the organic silicone insulating adhesive of the present invention is simple, the reaction conditions are mild, and it is easy to mass produce. The organic silicone insulating adhesive is applied to IBC batteries to avoid short circuits caused by thickness changes of the organic silicone insulating adhesive during welding of solder strips and lamination. The organic silicone insulating adhesive has excellent bonding strength with the adhesive film, thereby increasing the reliability of the components, which is conducive to further promoting the application of organic silicone insulating adhesive in the field of IBC batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1Schematic diagram of the distribution of the positive main grid line, positive fine sub-grid line, negative main grid line and negative fine sub-grid line on the back of the IBC battery.

[0037] Figure 2 for Figure 1 A partial enlarged schematic diagram of .

[0038] Figure 3 Schematic diagram of the structure of IBC battery.

[0039] In the figure, 1-silicon substrate, 2-n+ diffusion layer, 3-first passivation layer, 4-first anti-reflection layer, 5-local p+ diffusion layer, 6-local n+ diffusion layer, 7-second passivation layer, 8-second anti-reflection layer, 9-positive electrode, 901-positive electrode main grid line, 902-positive electrode auxiliary fine grid line, 903-high hardness silicone insulating glue, 10-negative electrode, 1001-negative electrode main grid line, 1002-negative electrode auxiliary fine grid line. DETAILED DESCRIPTION

[0040] The present invention is further described below in conjunction with specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.

[0041] Example 1

[0042] like Figure 3 As shown, the IBC battery includes a silicon substrate 1, an n+ diffusion layer 2 arranged on the front side of the silicon substrate 1, a first passivation layer 3 arranged on the n+ diffusion layer 2, a first anti-reflection layer 4 arranged on the first passivation layer 3, a local n+ diffusion layer 6 and a local p+ diffusion layer 5 arranged on the back side of the silicon substrate 1, a second passivation layer 7 arranged on the local n+ diffusion layer 6 and the local p+ diffusion layer 5, a second anti-reflection layer 8 arranged on the second passivation layer 7, a positive electrode 9 and a negative electrode 10 arranged on the second anti-reflection layer 8, the positive electrode 9 is electrically connected to the local p+ diffusion layer 5, and the negative electrode 10 is electrically connected to the local n+ diffusion layer 6;

[0043] like Figure 1 and Figure 2 As shown, the positive electrode 9 includes a positive electrode main grid line 901 and a positive electrode auxiliary fine grid line 902, and the negative electrode 10 includes a negative electrode main grid line 1001 and a negative electrode auxiliary fine grid line 1002. The positive electrode main grid line 901 is perpendicular to the positive electrode auxiliary fine grid line 902, and the negative electrode main grid line 1001 is perpendicular to the negative electrode auxiliary fine grid line 1002. The positive electrode auxiliary fine grid line 902 and the negative electrode auxiliary fine grid line 1002 are arranged in a forked finger shape, and the end of the positive electrode auxiliary fine grid line 902 does not contact the negative electrode main grid line 1001, and the end of the negative electrode auxiliary fine grid line 1002 does not contact the positive electrode main grid line 901, and the end of the positive electrode auxiliary fine grid line 902 and the end of the negative electrode auxiliary fine grid line 1002 are coated with a high-hardness organic silicon insulating glue 903;

[0044] The components of the high-hardness organic silicone insulating adhesive and the mass fractions of each component are as follows: 65 parts of polymethylvinylsiloxane, 10 parts of pretreated glass fiber (diameter ~ 25 μm and length ~ 5 mm, the same below), 10 parts of modified silica (particle size ~ 7 μm, the same below), 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol;

[0045] The pretreatment steps of the pretreated glass fiber are as follows: firstly, the glass fiber is placed at 700° C. for 30 minutes, then immersed in a 2% by mass silane coupling agent aqueous solution for 15 minutes, and finally baked at 100° C. for 10 minutes, thereby completing the pretreatment of the glass fiber;

[0046] The modified silica is obtained by the following method: 150 g of silica, 0.3 mol of propylene oxide, 0.03 mol of boron trifluoride etherate and 60 mL of dichloromethane are added into a flask, reacted at -20°C for 5 hours under a nitrogen atmosphere, then returned to room temperature and allowed to stand for 24 hours to obtain hydroxylated modified silica.

[0047] The preparation steps of the high-hardness organic silicone insulating adhesive are as follows: first, polymethylvinylsiloxane, pretreated glass fiber, modified silica, γ-aminopropyltriethoxysilane, polymethylhydrogensiloxane and polyvinyl alcohol are added into a mixer, and stirred at a stirring rate of 60 rpm for 15 minutes at 40°C to obtain a primary mixture; then, silane coupling agent KH-560 is added into the primary mixture, and stirred at a stirring rate of 30 rpm for 20 minutes at 50°C to obtain a secondary mixture; finally, vinyltriamine is added into the secondary mixture, and stirred at a stirring rate of 30 rpm for 20 minutes at 50°C to obtain the high-hardness organic silicone insulating adhesive.

[0048] Example 2

[0049] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the high hardness organic silicon insulating glue in Example 2 are as follows: 65 parts of polymethylvinylsiloxane, 15 parts of pretreated glass fiber, 5 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0050] Example 3

[0051] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the high hardness organic silicon insulating glue in Example 3 are as follows: 65 parts of polymethylvinylsiloxane, 5 parts of pretreated glass fiber, 15 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0052] Example 4

[0053] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the high hardness organic silicon insulating glue in Example 4 are as follows: 65 parts of polymethylvinylsiloxane, 15 parts of pretreated glass fiber, 15 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0054] Example 5

[0055] On the basis of Example 1, the content of each component in the high-hardness organic silicon insulating glue and its preparation process conditions are changed. Among them, the components of the high-hardness organic silicon insulating glue in Example 5 and the mass fractions of each component are as follows: 63 parts of polypropyl vinyl siloxane, 12 parts of pretreated glass fiber, 12 parts of modified calcium carbonate (particle size ~7μm), 4 parts of γ-glycidyloxypropyltrimethoxysilane, 2 parts of dimethylaminopropylamine, 0.8 parts of silane coupling agent KH-560, 4 parts of polyethyl hydrogen siloxane, and 2 parts of polyamide;

[0056] The pretreatment steps of the pretreated glass fiber are as follows: first, the glass fiber is placed at 650° C. for 25 minutes, then soaked in a 1% by mass silane coupling agent aqueous solution for 10 minutes, and finally baked at 110° C. for 10 minutes to complete the pretreatment of the glass fiber;

[0057] The modified calcium carbonate is obtained by the following method: 140 g of calcium carbonate, 0.18 mol of propylene oxide, 0.02 mol of boron trifluoride etherate and 55 mL of dichloromethane are added into a flask, reacted at -15°C for 6 hours under a nitrogen protective atmosphere, then returned to room temperature and allowed to stand for 20 hours to obtain hydroxylated modified calcium carbonate.

[0058] The preparation steps of the high hardness organic silicone insulating glue described in Example 5 are as follows: first, add polypropyl vinyl siloxane, pretreated glass fiber, modified calcium carbonate, γ-glycidyloxypropyltrimethoxysilane, polyethylhydrogensiloxane and polyamide into a blender, and stir at a stirring rate of 55 rpm for 20 minutes at 40°C to obtain a preliminary mixture; then add silane coupling agent KH-560 to the preliminary mixture, and stir at a stirring rate of 35 rpm for 25 minutes at 50°C to obtain a secondary mixture; finally, add dimethylaminopropylamine to the secondary mixture, and stir at a stirring rate of 35 rpm for 25 minutes at 50°C to obtain the high hardness organic silicone insulating glue.

[0059] Example 6

[0060] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the high hardness organic silicon insulating glue in Example 6 are as follows: 65 parts of polymethylvinylsiloxane, 20 parts of pretreated glass fiber, 0 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0061] Comparative Example 1

[0062] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the organic silicon insulating glue in Comparative Example 1 are as follows: 65 parts of polymethylvinylsiloxane, 0 parts of pretreated glass fiber, 0 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0063] Comparative Example 2

[0064] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the organic silicon insulating glue in Comparative Example 2 are as follows: 65 parts of polymethylvinylsiloxane, 0 parts of pretreated glass fiber, 20 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0065] Comparative Example 3

[0066] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the organic silicon insulating glue in Comparative Example 3 are as follows: 65 parts of polymethylvinylsiloxane, 2 parts of pretreated glass fiber, 2 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0067] Comparative Example 4

[0068] On the basis of Example 1, except for changing the content of each component in the high hardness organic silicon insulating glue, other conditions and preparation steps are the same as those in Example 1. Among them, the mass parts of each component in the organic silicon insulating glue in Comparative Example 4 are as follows: 65 parts of polymethylvinylsiloxane, 20 parts of pretreated glass fiber, 20 parts of modified silica, 5 parts of γ-aminopropyltriethoxysilane, 2 parts of vinyltriamine, 0.5 parts of silane coupling agent KH-560, 4.5 parts of polymethylhydrogensiloxane, and 3 parts of polyvinyl alcohol.

[0069] The organic silicon insulating adhesives obtained in Examples 1 to 6 and Comparative Examples 1 to 4 were respectively poured into a tetrafluoroethylene mold with a diameter of 100 mm and a depth of 1 mm, and then the mold was placed in an oven and baked at 150° C. for 20 min to obtain cured organic silicon insulating adhesive samples.

[0070] The volume resistivity of the silicone insulating adhesive sample was tested by an ultra-high resistance micro-ammeter. The test formula is ρ v =Rx(A / D),ρ v is the volume resistivity in Ω·m, Rx is the measured volume resistance of the sample in Ω, and A is the effective area of ​​the measuring electrode in m 2 , D is the thickness of the test sample, in m. To ensure measurement accuracy, a circular plate-shaped three-electrode system is generally used.

[0071] The pencil hardness of the cured silicone insulating film was measured according to GB / T 6739-2006 Test method for paint and varnish film hardness by pencil method.

[0072] The Shore hardness of the cured silicone insulating film was measured in accordance with GB / T 2411-2008 Plastics and hard rubber - Test method for indentation hardness using a hardness tester. The equipment used was a Shore D hardness tester.

[0073] The surface tension of the silicone insulating adhesive sample was measured using a dyne pen. The dyne value reflects the surface tension coefficient of the silicone insulating adhesive surface. The higher the dyne value, the greater the surface tension and the stronger the bonding strength between the silicone insulating adhesive and the film.

[0074] The peeling force (bonding strength) between silicone insulating adhesive and film is measured according to GB / T 2790-1995 Adhesive 180° Peel Strength Test Method Flexible Material to Rigid Material Test Method Standard, and the equipment used is a universal testing machine. The measurement method is to laminate the rigid adherend (silicone insulating adhesive), adhesive (film) and flexible adherend (backboard) and then test the peeling force on the universal testing machine.

[0075] The thermal decomposition temperature (when the thermal weight loss is 5%) of the silicone insulating adhesive sample was tested by a thermogravimetric analyzer. The test temperature range was 0 to 700°C. The test environment was carried out in a N2 atmosphere with a heating rate of 10°C / min.

[0076] The test results of volume resistivity, pencil hardness, Shore hardness, dyne value, peeling force between the insulating adhesive and the film, and thermal decomposition temperature of the silicone insulating adhesive are shown in Table 1.

[0077] Table 1

[0078]

[0079]

[0080] According to the test results of Comparative Example 1, when modified inorganic fillers and glass fibers are not added to the silicone insulating adhesive, the performance indicators of the silicone insulating adhesive are poor, the dyne value is only 6 dyne / cm, the peeling force between it and the adhesive film is only 2N, the pencil hardness is only 4B, and the Shore hardness is 45.

[0081] According to the test results of Comparative Example 2, adding hydroxylated silica to the silicone insulating adhesive can significantly improve the surface tension of the silicone insulating adhesive. The dyne value of the silicone insulating adhesive is increased to 28 dyne / cm, and the peeling force between the silicone insulating adhesive and the adhesive film is increased to 32N. However, it does not significantly improve the hardness of the insulating adhesive, with a pencil hardness of only 5B and a Shore hardness of 48.

[0082] According to the test results of Example 6, adding glass fiber to the silicone insulating adhesive can significantly improve the hardness of the silicone insulating adhesive. The pencil hardness of the silicone insulating adhesive is increased to 1H, and the Shore hardness is increased to 60. However, since no modified inorganic filler is added, the surface tension of the silicone insulating adhesive is not greatly improved. The dyne value of the insulating adhesive is 8dyne / cm, and the peeling force between it and the adhesive film is 6N.

[0083] According to the test results of Comparative Example 3, when too little modified inorganic filler and glass fiber are added to the silicone insulating adhesive, the improvement effect on the various performance indicators of the silicone is poor, the dyne value is 11 dyne / cm, the peeling force between it and the adhesive film is only 8N, the pencil hardness is only 5B, and the Shore hardness is 47.

[0084] According to the test results of Comparative Example 4, when too much modified inorganic filler and glass fiber are added to the silicone insulating adhesive, its hardness and bonding strength are not good, the dyne value is 30 dyne / cm, the peeling force between it and the adhesive film is 27N, the pencil hardness is 5B, and the Shore hardness is 56. This is mainly because excessive addition of glass fiber will cause steric hindrance between polyalkyl vinyl siloxane molecules, hindering intermolecular contact and crosslinking; and for inorganic fillers, excessive internal agglomeration will occur, which also hinders intermolecular crosslinking.

[0085] According to the test results of Examples 1 to 5, adding an appropriate amount of modified inorganic filler and glass fiber to the organosilicon insulating adhesive can not only increase the hardness of the organosilicon insulating adhesive, but also improve the surface tension of the organosilicon insulating adhesive and increase the bonding strength between it and the adhesive film. This is mainly attributed to the synergistic effect of the modified inorganic filler and the glass fiber. Since there are a large number of hydroxyl groups on the surface of the hydroxylated modified inorganic filler, some of these hydroxyl groups will migrate to the surface when blended with the glass fiber, making the hydroxyl groups more evenly dispersed on the surface of the organosilicon insulating adhesive, thereby effectively improving the surface tension of the organosilicon insulating adhesive, and its peeling force with the adhesive film is correspondingly increased; in addition, the modified inorganic filler and glass fiber can also be more evenly dispersed in the organosilicon insulating adhesive, because the particle size difference between the glass fiber and the modified inorganic filler is large, thereby avoiding agglomeration, and making the modified inorganic filler more evenly dispersed, which is conducive to further improving the hardness of the organosilicon insulating adhesive.

[0086] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An IBC battery, characterized in that: The invention comprises a positive main grid line, a positive fine sub-grid line, a negative main grid line and a negative fine sub-grid line distributed on the back of an IBC battery, wherein the positive main grid line is perpendicular to the positive fine sub-grid line, the negative main grid line is perpendicular to the negative fine sub-grid line, the positive sub-fine grid line and the negative sub-fine grid line are arranged in a forked finger shape, and the end of the positive sub-fine grid line does not contact the negative main grid line, and the end of the negative sub-fine grid line does not contact the positive main grid line, and the end of the positive sub-fine grid line and the end of the negative sub-fine grid line are both coated with a high-hardness organic silicon insulating glue; The high-hardness organic silicon insulating adhesive comprises components of polyalkyl vinyl siloxane and glass fiber, wherein the mass ratio of glass fiber to polyalkyl vinyl siloxane is less than or equal to 1:

4.

2. An IBC battery according to claim 1, characterized in that: The alkyl group in the polyalkylvinylsiloxane is an alkyl group having no more than 5 carbon atoms in the main chain; Or / and, the glass fiber has a diameter of 8 to 30 μm and a length of 3 to 20 mm.

3. An IBC battery according to claim 1, characterized in that: The glass fiber is pretreated before use by the following method: first, the glass fiber is burned at 600-800°C for 20-30 minutes, then soaked in a 0.5-3% by mass silane coupling agent aqueous solution for 10-15 minutes, and finally baked at 100-120°C for 10-15 minutes.

4. An IBC battery according to claim 1, characterized in that: The mass ratio of glass fiber to polyalkyl vinyl siloxane is 1:4 to 1:

14.

5. An IBC battery according to any one of claims 1 to 4, characterized in that: The components of the high-hardness organic silicon insulating adhesive also include modified inorganic fillers, wherein the mass ratio of the modified inorganic fillers to the glass fiber is 1:3 to 3:1, and the modified inorganic fillers are at least one of hydroxylated silica, calcium carbonate, alumina, magnesia and mica.

6. An IBC battery according to claim 5, characterized in that: The particle size of the modified inorganic filler is 5 to 10 μm; Or / and, the mass ratio of polyalkyl vinyl siloxane to the sum of glass fiber and modified inorganic filler is 2:1 to 3.5:

1.

7. An IBC battery according to claim 5, characterized in that: The modified inorganic filler is obtained by the following method: the inorganic filler, propylene oxide, boron trifluoride etherate and dichloromethane are mixed, reacted at -35 to -10°C for 4 to 6 hours under a protective atmosphere, then returned to room temperature, and then left for 10 to 25 hours to obtain a hydroxylated modified inorganic filler; The molar ratio of glycidol to boron trifluoride ether is 8:1-11:1, the concentration of glycidol in dichloromethane is 3-5 mol / L, and the concentration of the inorganic filler in dichloromethane is 2-3 g / mL.

8. An IBC battery according to claim 5, characterized in that: The components of the high-hardness organic silicon insulating adhesive also include at least one of an adhesion promoter, a curing agent, a silane coupling agent, an active monomer and a dispersant; The adhesion promoter is at least one of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane; The curing agent is at least one of ethylenetriamine, diethylenetriamine and dimethylaminopropylamine; The active monomer is at least one of polymethyl hydrogen siloxane, polyethyl hydrogen siloxane and polypropyl hydrogen siloxane; The dispersant is at least one of polyvinyl alcohol, polyamide and polyvinyl acetate; Among them, when the mass fraction of polyalkyl vinyl siloxane in the high hardness silicone insulating glue is 60 to 70 parts, the mass fraction of adhesion promoter is 3 to 5 parts, the mass fraction of curing agent is 1 to 3 parts, the mass fraction of silane coupling agent is 0.1 to 1 part, the mass fraction of active monomer is 4 to 8 parts, and the mass fraction of dispersant is 1 to 5 parts.

9. An IBC battery according to claim 8, characterized in that: The components of the high-hardness organic silicone insulating adhesive and the mass fractions of each component are as follows: 60-70 parts of polyalkyl vinyl siloxane, 5-15 parts of glass fiber, 5-15 parts of modified inorganic filler, 3-5 parts of adhesion promoter, 1-3 parts of curing agent, 0.1-1 part of silane coupling agent, 4-8 parts of active monomer, and 1-5 parts of dispersant.

10. An IBC battery according to claim 9, characterized in that: The high-hardness organic silicon insulating adhesive is prepared by the following method: First, polyalkyl vinyl siloxane, glass fiber, modified inorganic filler, adhesion promoter, active monomer and dispersant are mixed evenly to obtain a primary mixture; then a silane coupling agent is added and mixed evenly to obtain a secondary mixture; finally, a curing agent is added and mixed evenly to obtain the high-hardness organic silicone insulating adhesive.

11. An IBC battery according to claim 10, characterized in that: In the process of obtaining the preliminary mixture, the stirring temperature is 30-40°C, the stirring rate is 50-80 rpm, and the stirring time is 15-20 min; In the process of adding the silane coupling agent to obtain the secondary mixture, the stirring temperature is 50-60° C., the stirring rate is 30-40 rpm, and the stirring time is 20-30 min; In the process of adding the curing agent to obtain the high-hardness organic silicon insulating adhesive, the stirring temperature is 50-60° C., the stirring speed is 30-40 rpm, and the stirring time is 20-30 min.

12. An IBC battery according to claim 1, characterized in that: The IBC cell further includes a silicon substrate, an n+ diffusion layer disposed on the front side of the silicon substrate, a first passivation layer disposed on the n+ diffusion layer, a first anti-reflection layer disposed on the first passivation layer, a local n+ diffusion layer and a local p+ diffusion layer disposed on the back side of the silicon substrate, a second passivation layer disposed on the local n+ diffusion layer and the local p+ diffusion layer, a second anti-reflection layer disposed on the second passivation layer, and a positive electrode and a negative electrode disposed on the second anti-reflection layer, wherein the positive electrode is electrically connected to the local p+ diffusion layer, and the negative electrode is electrically connected to the local n+ diffusion layer; The positive electrode includes the positive electrode main grid line and the positive electrode auxiliary fine grid line; the negative electrode includes the negative electrode main grid line and the negative electrode auxiliary fine grid line.

Citation Information

Patent Citations

  • Room-temperature cured insulating coating material and preparation method thereof

    CN111057465A

  • Insulating glue, preparation method of insulating glue and IBC solar cell

    CN111635725A

  • Insulating paste for IBC solar cell and preparation method thereof

    CN116515435A

  • Low-temperature welded back contact photovoltaic module and preparation method thereof

    CN116995109A

  • IBC battery structure

    CN206602118U

Cited By

  • Photovoltaic module

    CN122180153A