Method for preparing sintering enhancer by using high-iron steel slag

By acid leaching the magnetic tailing slag and mixing it with the reinforcement regulator, the problems of low utilization rate of steel slag and limited application are solved, the strength and combustion efficiency of sintered ore are improved, and the high-speed steel slag is realized. Resource utilization.

CN118957180AActive Publication Date: 2024-11-15NORTHEASTERN UNIV CHINA

Patent Information

Application Number
CN202411050217.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The low utilization rate of steel slag leads to waste of resources and environmental pollution, and its application in sintering processes is limited by poor tissue stability and unreasonable components.

Method used

By acid-leaching the magnetic separation tail slag after magnetic separation, the sintering reinforcement is prepared by washing the silicon and mixing it with the reinforcement regulator to reduce the silicon content to increase the proportion of iron components, simplify the process flow and reduce costs.

Benefits of technology

It improves the strength and combustion efficiency of sintered ore, reduces the cost of sintered ingredients, solves the problems of steel slag tail slag accumulation and application, and realizes the resource utilization of high-speed steel slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957180A_ABST
    Figure CN118957180A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a sintering enhancer by using high-iron steel slag, which comprises the following steps of: treating converter steel slag in manners of hot disintegration, hot splashing, tray treatment, air quenching, water quenching and the like, and performing magnetic separation to obtain magnetic separation tailings; after magnetic separation tailings are ground, calcium and magnesium are leached out in an acid solution, and leaching liquid and leaching tailings are obtained through filtering; adding an acid solution into the leaching tailings, stirring and reacting for 1-4 hours at the temperature of 10-50 DEG C, and filtering and drying after solid-liquid layering to obtain a sintering enhancer master batch; the sintering enhancer master batch and the enhancement regulating agent are respectively ground into powder, and the powder is mixed in proportion to prepare a mixture with binary alkalinity of 1.5-3, namely the final sintering enhancer. According to the method, the raw materials are easy to obtain, the process is simple, operation is convenient, the obtained product can be directly added into the sintering raw materials, good sintering strength can be provided for the sintered ore, and meanwhile the sintering ingredient cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of comprehensive utilization of metallurgical resources, and specifically relates to a method for preparing a sintering intensifier by utilizing high-iron steel slag. Background Art

[0002] According to statistics from the World Steel Association, in 2023, my country's crude steel output will be 1.019 billion tons, accounting for about 54% of the world's total output. Steel slag is an inevitable solid waste produced in the steelmaking process. In 2023 alone, my country produced more than 100 million tons of steel slag. At present, the utilization rate of steel slag in Europe and the United States has reached 90%, while the utilization rate of steel slag in China is between 20% and 30%. Due to the low comprehensive utilization rate of steel slag in my country, more than hundreds of millions of tons of steel slag are stored, occupying a large amount of space and land, and there is a high possibility of ecological risks such as leaching of toxic heavy metal elements and pollution of surrounding water and soil. Therefore, how to select a suitable ecological disposal method based on its characteristics so that steel slag can be fully utilized as a resource has become a major issue of concern in the metallurgical industry.

[0003] Domestic steel enterprises mainly adopt methods such as hot stuffing, hot pouring, shallow pan, wind quenching, and water quenching to treat steel slag, and rarely carry out deep processing and value-added treatment. Steel slag contains a large amount of Fe, Ca and other components, and is an ideal raw material for sintering enhancers. Since the Fe component in the slag is easily combined with the Ca component to form calcium ferrite, it affects the efficiency of magnetic separation recovery, resulting in a common situation where the Fe content of magnetic separation tailings is high. If it is not handled properly, it will directly cause a waste of resources, and also affect the application of steel slag in civil engineering fields such as cementitious materials. Previous studies have shown that the free calcium oxide phase in steel slag can be selectively decomposed by treating steel slag with an acidic solution, and the calcium-containing solution can be used to capture CO2 in metallurgical flue gas, realizing waste treatment with waste. At the same time, the stability of the treated steel slag is greatly improved, and the calcium ferrite is enriched, which is an ideal masterbatch for preparing sintering enhancers. Compared with other sintering intensifiers, extracting valuable components from waste generated in the metallurgical process and applying them to the recycling process can realize the resource utilization of high-iron (high Fe component content) steel slag and avoid large-scale mining of related mineral resources.

[0004] At present, the utilization of steel slag still has the following problems that are difficult to solve: first, the components and elements in steel slag are numerous and complex, making it difficult to selectively extract and utilize them in stages; second, the tailings contain free CaO and MgO, and calcium silicate is in a metastable phase after rapid cooling, resulting in poor structural stability of the tailings; third, the tailings are dense and hard, with poor grindability, and the grinding cost of preparing steel slag micropowder is high, which reduces the economic efficiency of utilization. Therefore, the use of steel slag is mainly limited by poor structural stability and unreasonable components. Patent CN114293010A discloses a method for preparing sintered ore by adding steel slag tailings to a sintering process. The preparation of raw materials in this method requires the participation of multiple materials, and the batching is relatively difficult. Patent CN 116891938 A discloses a method for preparing sintered ore using converter steel slag tailings. The application is to mix iron materials with ingredients, use a pelletizer to make pellets for the sintering process, and then use distribution equipment, ignition and sintering to finally obtain sintered ore; but it needs to go through the steps of pelletizing, distribution, sintering, etc., and cannot directly obtain sintered ore. Patent CN116287687A discloses a method for preparing sintered ore using steel slag tailings after CaO extraction. The application is to mix steel slag tailings obtained after CaO extraction, fine iron ore, iron ore powder and other raw materials with water and granulate them, and then burn the mixed material to obtain sintered material; but it does not explain whether the extraction of CaO will affect the strength of the sintered ore and other factors. Patent CN 116574901A discloses a granulation intensifier, sintering mixture and super-thick material layer sintering intensification method based on metallurgical solid waste. The application prepares a granulation intensifier by using metallurgical solid waste, and then uses the prepared granulation intensifier as one of the raw materials to prepare a sintering mixture; however, the granulation intensifier cannot be directly added to the sintered ore, and the finished products of the granulation intensifier and the sintering mixture have high requirements and strict process requirements. Summary of the invention

[0005] In order to overcome the defects of the above-mentioned prior art and solve the problem of steel slag tailings accumulation and its application in the sintering process, the present invention performs acid leaching on the magnetic separation tailings after magnetic separation, washes the silicon and mixes it with a strengthening regulator to obtain a sintering strengthener; this method has the characteristics of simple raw materials, simple process, and convenient operation, and the obtained product can be directly added to the sintering raw materials without further sintering the sintering strengthener; by reducing the silicon content in the magnetic separation tailings to increase the proportion of iron components, it can provide good sintering strength for the sintered ore and also reduce the sintering ingredient cost.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing a sintering enhancer using high-iron steel slag, the method comprising the following steps:

[0007] ① In the converter smelting production process, after the converter slag is discharged, the converter slag is treated by hot stuffing, hot pouring, shallow pan, air quenching, water quenching, etc., and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings;

[0008] ② Grind the magnetic separation tailings obtained in step ①, leach them in an acidic solution, and filter to obtain a leachate and leached tailings;

[0009] ③ Add an acidic solution to the leaching tailings obtained in step ②, stir and react at 10° C. to 50° C. for 1 to 4 hours, filter and dry after solid-liquid separation to obtain a sintering enhancer masterbatch;

[0010] ④ Grind the sintering enhancer masterbatch and the enhancing regulator obtained in step ③ into powder respectively, mix them according to proportion, and obtain a mixture with a binary basicity of 1.5 to 3, which is the final sintering enhancer.

[0011] The main phases of the converter slag are dicalcium silicate, metallic iron phase, free calcium oxide, calcium aluminoferrite and ferrite, wherein the Fe content is greater than 15%, and the main components are CaO, SiO2, FeO, MgO, Al2O3 and the like.

[0012] In the above technical scheme, further, the magnetic separation tailings obtained in step ① are used as raw materials for preparing sintering intensifiers, and the mass fractions of the main chemical components in the raw materials are as follows: TFe: 15% to 25%, CaO mass fraction is 40% to 60%, SiO2 mass fraction is 10% to 20%, and MgO mass fraction is 6% to 10%.

[0013] Furthermore, in step ②, the acidic solution is a solution of one or more configurations of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, ammonium sulfate, etc., the pH value is 2-3, and the concentration of the acidic solution is 0.5-2 mol / L; the leaching reaction temperature is 10°C-100°C, the leaching reaction time is 0.5-4h, and the leaching stirring rate is 150-600rpm; the solid-liquid ratio of the magnetic separation tailings to the acidic solution is 1:5-1:40g / mL.

[0014] Furthermore, in step ②, the obtained leaching tailings are made into cylindrical materials by a mold, and the materials are sent to a heating device to observe the melting morphology of the materials, and the melting point and melting rate of the leaching tailings are measured, so as to judge whether the obtained sintering enhancer meets the sintering conditions according to these conditions. The mass fractions of the main chemical components of the leaching tailings in step ② are TFe: 20% to 40%, CaO (or other Ca compounds): 20% to 30%, SiO2: 25% to 35%, and MgO: 2% to 6%.

[0015] Furthermore, in step ③, the acidic solution system is a solution of one or more of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, ammonium sulfate, etc., with a pH value of 0.1-1, and a concentration of the acidic solution of 0.5-1 mol / L; the solid-liquid ratio of the leaching tailings to the acidic solution is 1:5-1:40 g / mL, and the stirring rate is 300-600 rpm.

[0016] Furthermore, in step ④, the strengthening regulator is one or two of CaO reagent and SiO2 reagent, and the dried strengthening agent masterbatch and the strengthening regulator are respectively ground into powders less than 100 mesh, and the strengthening agent masterbatch and the strengthening regulator are mixed into a mixture with a binary basicity (CaO / SiO2) of 1.5 to 3 in a mass ratio of 1:0.25 to 1:0.5. The sintering strengthener prepared under this basicity condition can provide good sintering strength for the sintered ore.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention uses steel slag tailings with high iron and calcium content to complete the preparation of a sintering intensifier, increases the proportion of iron by reducing the silicon content in the high-iron steel slag, maximizes the use of the iron phase in the steel slag tailings, effectively improves combustion efficiency, reduces the amount of solid fuel used, increases the strength of sintered ore, and promotes iron increase and coke saving in blast furnaces.

[0019] In this technical solution, the prepared raw materials and strengthening regulators are dried, and no water is added during the raw material preparation and raw material configuration process, thus avoiding the influence of water on the sintering strengthener. The converter slag after magnetic separation is acid-leached, washed with silicon and mixed with the strengthening regulator to obtain the sintering strengthener; this method has the characteristics of simple raw materials, simple process, and convenient operation, and the obtained sintering strengthener can be directly added to the sintering raw materials without further sintering of the sintering strengthener; it can provide good sintering strength for the sintered ore, and at the same time reduce the cost of sintering ingredients, solving the problem of steel slag tailings accumulation and its application in the sintering process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The process flow chart of the method for preparing a sintering enhancer by using high-speed iron slag of the present invention;

[0021] Figure 2 The XRD diagram of the magnetic separation tailings in step ① of Example 1;

[0022] Figure 3 This is the XRD diagram of the leached tailings described in step ② in Example 1. DETAILED DESCRIPTION

[0023] In order to more clearly present the technical features and beneficial effects of the present invention, the following embodiments and drawings will be specifically described. It should be understood by those skilled in the art that the following embodiments are only used to illustrate the present invention and are not intended to limit the present invention in any way.

[0024] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents, materials, instruments and equipment, etc., are all commercially available unless otherwise specified.

[0025] A method for preparing a sintering enhancer using high-iron steel slag, the method comprising the following steps:

[0026] ① In the converter smelting production process, after the converter is slaged, the converter slag is treated by hot stuffing, hot pouring, shallow pan, wind quenching, water quenching, etc., and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 15%~25%, CaO: 40%~60%, SiO2: 10%~20%, MgO: 6%~10%.

[0027] ② After grinding the magnetic separation tailings obtained in step ①, leaching in an acidic solution, filtering to obtain a leachate and leached tailings; the solid-liquid ratio of the magnetic separation tailings to the acidic solution is 1:5-1:40 g / mL; the leaching temperature is 10°C-100°C, the reaction time is 0.5-4h, and the stirring rate is 150-600rpm. The acidic solution in step ② is a solution of one or more of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, and ammonium sulfate, with a solution concentration of 0.5-2 mol / L and a pH value of 2-3. The mass fraction of the main chemical components of the leached tailings in step ② is TFe: 20%-40%, CaO: 20%-30%, SiO2: 25%-35%, and MgO: 2%-6%.

[0028] ③ Add an acidic solution to the leached tailings obtained in step ②, stir the reaction at 10° C. to 50° C. for 1 to 4 hours, filter and dry after solid-liquid stratification to obtain a sintering enhancer masterbatch; the acidic solution in step ③ is a solution prepared by one or more of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, and ammonium sulfate, with a pH value of 0.1 to 1, and a concentration of the acidic solution of 0.5 to 1 mol / L; the solid-liquid ratio of the leached tailings to the acidic solution in step ③ is 1:5 to 1:40 g / mL, and the stirring rate is 300 to 600 rpm.

[0029] ④ Grind the sintering enhancer masterbatch and the enhancing regulator obtained in step ③ into powder respectively, mix them in proportion, and prepare a mixture with a binary basicity of 1.5 to 3, which is the final sintering enhancer. The enhancing regulator in step ④ is one or two of CaO reagent and SiO2 reagent. Grind the dried enhancer masterbatch and the enhancing regulator into powders of less than 100 mesh respectively, and prepare the enhancer masterbatch and the enhancing regulator into a mixture in a mass ratio of 1:0.25 to 1:0.5.

[0030] The matters not described in the following embodiments are the same as the description of the above specific implementation methods.

[0031] Example 1

[0032] A method for preparing a sintering enhancer using high-speed iron slag, the specific process flow is:

[0033] ① In the converter smelting production process, after the converter slag is discharged, the converter slag is treated by hot stuffing and hot pouring, and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 20%, CaO: 50%, SiO2: 15%, MgO: 9% by mass; the XRD diagram of the magnetic separation tailings is as follows Figure 2 As shown by Figure 2 It can be seen that the iron oxide phase and the calcium silicate phase are the main phases.

[0034] ② Grind the magnetic separation tailings obtained in step ① to make the particle size less than 100 mesh, and place the magnetic separation tailings in an acidic solution (acetic acid solution) with a concentration of 1 mol / L, wherein the solid-liquid ratio of the magnetic separation tailings to the acetic acid solution is 1:5 g / mL, the reaction temperature is 20°C, the reaction time is 2h, and the stirring rate is 300rpm; after filtering, the leaching liquid and leaching tailings are obtained. The XRD pattern of the leaching tailings in step ② is as follows Figure 3 As shown by Figure 3 It can be seen that the iron oxide phase is still the main phase, but the calcium silicate phase is significantly reduced, which proves that the selective leaching of calcium has been achieved and the proportion of iron has been increased.

[0035] The main chemical components of the leaching tailings in step ② are TFe: 29%, CaO: 24%, SiO2: 29%, and MgO: 2%.

[0036] The leaching tailings obtained in step ② were molded into cylindrical materials with a diameter and height of 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials, and the melting point was measured to be 1201°C.

[0037] The leaching tailings obtained in step ② were molded into cylindrical materials. The diameter and height of the materials were set to 3 mm. The materials were sent into a heating device to observe the melting morphology characteristics of the materials. The measured melting rate was 106 s.

[0038] ③ Add an acidic solution (hydrochloric acid solution) to the leached tailings obtained in step ②, the concentration of the hydrochloric acid solution is 1 mol / L, the solid-liquid ratio of the leached tailings to the hydrochloric acid solution is 1:20 g / mL, the reaction temperature is 20 ° C, the reaction time is 2 h, the stirring rate is 300 rpm, and after solid-liquid stratification, filter and dry to obtain a sintering enhancer masterbatch.

[0039] ④ The dried strengthener masterbatch (iron ore powder) and strengthening regulator (CaO) reagent obtained in step ③ are respectively ground into powders less than 100 mesh, and the iron ore powder and CaO reagent are prepared into a mixture with a binary basicity of 2.0 according to a mass ratio of 1:0.38, and finally a sintering strengthener is obtained. The mass fractions of the components of the sintering strengthener and magnetic separation tailings finally obtained in Example 1 are shown in Table 1. It can be seen from Table 1 that this process ultimately increases the proportion of the Fe component, and the final product sintering strengthener can provide good sintering strength for the sintered ore, and the parameter effect of Example 1 is better.

[0040] Example 2

[0041] A method for preparing a sintering enhancer using high-speed iron slag, the specific process flow is:

[0042] ① In the converter smelting production process, after the converter slag is discharged, the converter slag is treated by hot stuffing and hot pouring, and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 20%, CaO: 50%, SiO2: 15%, and MgO: 9% by mass.

[0043] ② Grind the magnetic separation tailings obtained in step ① to make the particle size less than 100 mesh, place the magnetic separation tailings in an acidic solution (acetic acid solution) with a concentration of 1 mol / L, wherein the solid-liquid ratio of the magnetic separation tailings to the acetic acid solution is 1:5 g / mL, the reaction temperature is 20° C., the reaction time is 2 h, and the stirring rate is 300 rpm; filter to obtain a leachate and a leach tailing; the mass fractions of the main chemical components of the leach tailings are TFe: 27%, CaO: 25%, SiO2: 30%, and MgO: 3%.

[0044] The leaching tailings obtained in step ② were molded into cylindrical materials with a diameter and height of 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials, and the melting point was measured to be 1204°C.

[0045] The leaching tailings obtained in step ② were molded into cylindrical materials. The diameter and height of the materials were set to 3 mm. The materials were sent into a heating device to observe the melting morphology characteristics of the materials. The measured melting rate was 115 s.

[0046] ③ Add an acidic solution (hydrochloric acid solution) to the leached tailings obtained in step ②, the concentration of the hydrochloric acid solution is 1 mol / L, the solid-liquid ratio of the leached tailings to the hydrochloric acid solution is 1:20 g / mL, the reaction temperature is 20 ° C, the reaction time is 2 h, the stirring rate is 300 rpm, the mixed solution is reacted for a period of time, and after solid-liquid stratification, it is filtered and dried to obtain a sintering enhancer masterbatch.

[0047] ④ Grind the dried strengthener masterbatch (iron ore powder) and strengthening regulator (CaO) obtained in step ③ into powders of less than 100 mesh, and mix the iron ore powder and CaO reagent into a mixture with a binary basicity of 2.0 in a mass ratio of 1:0.38 to finally prepare a sintering strengthener. Example 2 The mass fractions of the components of the sintering strengthener finally prepared are shown in Table 1.

[0048] Example 3

[0049] A method for preparing a sintering enhancer using high-speed iron slag, the specific process flow is:

[0050] ① In the converter smelting production process, after the converter is slaged, the converter slag is treated by hot stuffing and hot pouring, and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 20%, CaO: 50%, SiO2: 15%, and MgO: 9% by mass.

[0051] ② Grind the magnetic separation tailings obtained in step ① to make the particle size less than 100 mesh, place the magnetic separation tailings in an acidic solution (acetic acid solution) with a concentration of 2 mol / L, wherein the solid-liquid ratio of the magnetic separation tailings to the acetic acid solution is 1:5 g / mL, the reaction temperature is 20° C., the reaction time is 2 h, and the stirring rate is 300 rpm; after filtering, a leachate and a leach tailing are obtained, wherein the mass fractions of the main chemical components of the leach tailings are TFe: 28%, CaO: 25%, SiO2: 28%, and MgO: 4%.

[0052] The leaching tailings obtained in step ② were molded into cylindrical materials with a diameter and height of 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials, and the melting point was measured to be 1205°C.

[0053] The leaching tailings obtained in step ② were molded into cylindrical materials. The diameter and height of the materials were set to 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials. The measured melting rate was 112 s.

[0054] ③ Add an acidic solution (hydrochloric acid solution) to the leached tailings obtained in step ②, the concentration of the hydrochloric acid solution is 1 mol / L, the solid-liquid ratio of the leached tailings to the hydrochloric acid solution is 1:20 g / mL, the reaction temperature is 20 ° C, the reaction time is 2 h, the stirring rate is 300 rpm, the mixed solution is reacted for a period of time, and after solid-liquid stratification, it is filtered and dried to obtain a sintering enhancer masterbatch.

[0055] ④ Grind the dried strengthener masterbatch (iron ore powder) and strengthening regulator (CaO) obtained in step ③ into powders of less than 100 mesh, and mix the iron ore powder and CaO reagent into a mixture with a binary basicity of 2.0 in a mass ratio of 1:0.38 to finally prepare a sintering strengthener. Example 3 The mass fractions of the components of the sintering strengthener finally prepared are shown in Table 1.

[0056] Example 4

[0057] A method for preparing a sintering enhancer using high-speed iron slag, the specific process flow is:

[0058] ① In the converter smelting production process, after the converter is slaged, the converter slag is treated by hot stuffing and hot pouring, and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 20%, CaO: 50%, SiO2: 15%, and MgO: 9% by mass.

[0059] ② Grind the magnetic separation tailings obtained in step ① to make the particle size less than 100 mesh, place the magnetic separation tailings in an acidic solution (acetic acid solution) with a concentration of 1 mol / L, wherein the solid-liquid ratio of the magnetic separation tailings to the acetic acid solution is 1:5 g / mL, the reaction temperature is 20° C., the reaction time is 2 h, and the stirring rate is 300 rpm; after filtering, a leachate and a leach tailing are obtained, wherein the mass fractions of the main chemical components of the leach tailings are TFe: 25%, CaO: 26%, SiO2: 30%, and MgO: 6%.

[0060] The leaching tailings obtained in step ② were molded into cylindrical materials with a diameter and height of 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials, and the melting point was measured to be 1201°C.

[0061] The leaching tailings obtained in step ② were molded into cylindrical materials. The diameter and height of the materials were set to 3 mm. The materials were sent into a heating device to observe the melting morphology characteristics of the materials. The measured melting rate was 106 s.

[0062] ③ Add an acidic solution (hydrochloric acid solution) to the leached tailings obtained in step ②, the concentration of the hydrochloric acid solution is 2 mol / L, the solid-liquid ratio of the leached tailings to the hydrochloric acid solution is 1:5 g / mL, the reaction temperature is 20 ° C, the reaction time is 2 h, the stirring rate is 300 rpm, the mixed solution is reacted for a period of time, and after solid-liquid stratification, it is filtered and dried to obtain a sintering enhancer masterbatch.

[0063] ④ Grind the dried strengthener masterbatch (iron ore powder) and strengthening regulator (CaO) obtained in step ③ into powders of less than 100 mesh, and mix the iron ore powder and CaO reagent into a mixture with a binary basicity of 2.0 in a mass ratio of 1:0.38 to finally prepare a sintering strengthener. Example 4 The mass fractions of the components of the sintering strengthener finally prepared are shown in Table 1.

[0064] Example 5

[0065] A method for preparing a sintering enhancer using high-speed iron slag, the specific process flow is:

[0066] ① In the converter smelting production process, after the converter is slaged, the converter slag is treated by hot stuffing and hot pouring, and then the converter slag enters the magnetic separation line for magnetic separation to obtain magnetic separation tailings; the main chemical components of the magnetic separation tailings are TFe: 20%, CaO: 50%, SiO2: 15%, and MgO: 9% by mass.

[0067] ② Grind the magnetic separation tailings obtained in step ① to make the particle size less than 100 mesh, place the magnetic separation tailings in an acidic solution (acetic acid solution) with a concentration of 1 mol / L, wherein the solid-liquid ratio of the magnetic separation tailings to the acetic acid solution is 1:5 g / mL, the reaction temperature is 20° C., the reaction time is 2 h, and the stirring rate is 300 rpm; after filtering, a leachate and a leach tailing are obtained, wherein the mass fractions of the main chemical components of the leach tailings are TFe: 23%, CaO: 27%, SiO2: 30%, and MgO: 5%.

[0068] The leaching tailings obtained in step ② were molded into cylindrical materials with a diameter and height of 3 mm. The materials were sent into a heating device to observe the melting morphology of the materials, and the melting point was measured to be 1201°C.

[0069] The leaching tailings obtained in step ② were molded into cylindrical materials. The diameter and height of the materials were set to 3 mm. The materials were sent into a heating device to observe the melting morphology characteristics of the materials. The measured melting rate was 106 s.

[0070] ③ Add an acidic solution (hydrochloric acid solution) to the leached tailings obtained in step ②, the concentration of the hydrochloric acid solution is 1 mol / L, the solid-liquid ratio of the leached tailings to the hydrochloric acid solution is 1:10 g / mL, the reaction temperature is 20 ° C, the reaction time is 2 h, the stirring rate is 300 rpm, the mixed solution is reacted for a period of time, and after solid-liquid stratification, it is filtered and dried to obtain a sintering enhancer masterbatch.

[0071] ④ Grind the dried strengthener masterbatch (iron ore powder) and strengthening regulator (CaO) obtained in step ③ into powders of less than 100 mesh, and mix the iron ore powder and CaO reagent into a mixture with a binary basicity of 2.0 in a mass ratio of 1:0.38 to finally prepare a sintering strengthener. Example 5 The mass fractions of the components of the sintering strengthener finally prepared are shown in Table 1.

[0072] Table 1 Comparison of mass fractions of sintering enhancers and magnetic separation tailings obtained in Examples 1-5 (wt%)

[0073] Group TFe CaO <![CDATA[SiO2]]> MgO Magnetic separation tailings 20 50 15 9 Example 1 44 29 11 3 Example 2 40 25 13 4 Example 3 32 30 14 7 Example 4 36 32 13 6 Example 5 39 31 14 5

[0074] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a sintering enhancer using high-iron steel slag, characterized in that: The method comprises the following steps: ① Treat the converter slag by hot stuffing, hot pouring, shallow pan, air quenching, and water quenching, and then perform magnetic separation to obtain magnetic separation tailings; ② Grind the magnetic separation tailings obtained in step ①, leach them in an acidic solution, and filter to obtain a leachate and leached tailings; ③ Add an acidic solution to the leaching tailings obtained in step ②, stir and react at 10° C. to 50° C. for 1 to 4 hours, filter and dry after solid-liquid separation to obtain a sintering enhancer masterbatch; ④ Grind the sintering enhancer masterbatch and the enhancing regulator obtained in step ③ into powder respectively, mix them according to proportion, and prepare a mixture with a binary basicity of 1.5 to 3, which is the final sintering enhancer.

2. The method according to claim 1, characterized in that: In step ①, the main chemical components of the magnetic separation tailings are TFe: 15% to 25%, CaO: 40% to 60%, SiO2: 10% to 20%, and MgO: 6% to 10%.

3. The method according to claim 2, characterized in that Step ② The acidic solution is a solution of one or more of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, and ammonium sulfate, with a solution concentration of 0.5 to 2 mol / L and a pH value of 2 to 3.

4. The method according to claim 3, characterized in that In step ②, the solid-liquid ratio of the magnetic separation tailings to the acidic solution is 1:5-1:40 g / mL; the leaching temperature is 10° C.-100° C., the reaction time is 0.5-4 h, and the leaching stirring rate is 150-600 rpm.

5. The method according to claim 4, characterized in that The main chemical components of the leaching tailings in step ② are TFe: 20% to 40%, CaO: 20% to 30%, SiO2: 25% to 35%, and MgO: 2% to 6%.

6. The method according to claim 5, characterized in that Step ③: the acidic solution is a solution prepared by one or more of formic acid, acetic acid, hydrochloric acid, sulfuric acid, ammonium chloride, ammonium nitrate, and ammonium sulfate, with a pH value of 0.1 to 1 and a concentration of 0.5 to 1 mol / L.

7. The method according to claim 6, characterized in that In step ③, the solid-liquid ratio of the leaching tailings to the acidic solution is 1:5-1:40 g / mL, and the stirring rate is 300-600 rpm.

8. The method according to claim 7, characterized in that In step ④, the strengthening regulator is one or both of a CaO reagent and a SiO2 reagent. The dried strengthening agent masterbatch and the strengthening regulator are respectively ground into powders of less than 100 meshes, and the strengthening agent masterbatch and the strengthening regulator are prepared into a mixed material in a mass ratio of 1:0.25 to 1:0.5.

Citation Information

Patent Citations

  • Calcium-magnesium sintering additive and production process flows thereof

    CN102899481A

  • Method for recovering iron in steel slag and using tailing thereof

    CN105714003A

  • Efficient resource utilization method of converter steel slag

    CN110499400A

  • Metallurgy sintering synergist as well as preparation method and application thereof

    CN114438312A

  • Environment-friendly treatment method for industrial waste dephosphorized steel slag

    CN115057475A

Cited By

  • Integrated purification reaction equipment for treating steel tailings

    CN121718659A