Method for slow cooling and carbon sequestration of pyrogenic process smelting slag
By combining carbon dioxide gas purge and water quenching cooling, the problems of high energy consumption, large water consumption and long cooling time in the slow cooling process of ignition smelting slag are solved, and efficient separation and recovery of metals such as iron and copper are achieved. , the carbon dioxide fixation rate is high, and it is suitable for the resource utilization of ignition smelting slag.
Patent Information
- Application Number
- CN202411181560.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
Copper and iron are difficult to separate in the slag of smelting by pyrotechnic method, and the recovery rate is low. The existing slow-cooling process has problems such as high energy consumption, large water consumption and long slow-cooling time. There is a lack of methods that can simultaneously shorten the slow-cooling time and promote the crystallization of metal minerals. .
The melting smelting slag is purged and cooled by using carbon dioxide gas to convert silicate minerals into carbonate minerals to produce silica, reduce viscosity and fluidity, promote the growth of iron and copper crystals, and is quenched to Room temperature, combined with mobile water mist cooling to further cool.
It significantly shortens the slow cooling time, improves the metal recovery rate, and the carbon dioxide fixation rate exceeds 85%, achieving efficient separation and recycling of metals such as iron and copper, with high economic benefits and suitable for industrial applications.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource utilization of industrial waste slag, and specifically relates to a method for slowly cooling and carbonizing slag from pyrometallurgical process. Background Art
[0002] Pyrometallurgical smelting is one of the important methods of metal smelting and an important part of carbon emissions. Pyrometallurgical slag is an alkaline solid waste produced by metal smelting. Due to the lack of suitable treatment and disposal methods (comprehensive utilization rate <10%), it is still mainly stored, which not only occupies a large amount of land but also pollutes the environment. In addition, the content of Cu and Fe in pyrometallurgical slag is relatively high. Taking copper smelting slag as an example, its main mineral phases are fayalite (2FeO·SiO 2 ), a small amount of magnetite (Fe 3 O 4 ) and matte (Cu 2 S~FeS solid solution), the iron and copper contents can reach 40% and 0.5~3% respectively, which are much higher than the grades of copper and iron ore mined in my country. It is regarded as a secondary resource with great value. However, due to the inter-embedded copper and iron minerals, they are difficult to separate, the recovery rate is low, and the economic value is low.
[0003] The key technical bottlenecks for the difficulty in separating copper and iron from pyrometallurgical slag and the low recovery rate are that copper, iron and other elements have low crystallinity and fine grains during the slow cooling process, and metal ions are embedded in each other during the mineral reconstruction process in the high-temperature molten state, making them difficult to separate subsequently.
[0004] The slow cooling process of molten pyrometallurgical slag includes air slow cooling and water quenching slow cooling, wherein air slow cooling can increase copper aggregation and crystallization state, the process flow is simple and the investment is low, but the slow cooling time is long, and the crystal size of copper minerals is small and uneven. Water quenching slow cooling greatly shortens the slow cooling time, but the water consumption is large, the metal minerals are interlocked, the crystallinity is extremely low, the energy consumption of iron and copper separation is high, and the recovery rate is low. At present, there is no new slow cooling process that can shorten the slow cooling time and promote the crystallization of metal minerals and increase the metal recovery rate. For this reason, it is very necessary to develop a method for slow cooling and carbon fixation of pyrometallurgical slag that can solve the above problems. Summary of the invention
[0005] The object of the present invention is to provide a method for slow cooling and carbon fixation of pyrometallurgical slag, which can shorten the slow cooling time and promote the crystallization of metal minerals, thereby increasing the metal recovery rate.
[0006] The object of the present invention is achieved by comprising the following steps: S1. Purging and slow cooling of molten pyrometallurgical slag: introducing carbon dioxide gas into a high-temperature stirring tank to purge and slowly cool the molten pyrometallurgical slag to obtain carbonized smelting slag; S2. Water quenching of carbonized smelting slag: cool the carbonized smelting slag to room temperature by water cooling.
[0007] Preferably, the silicate mineral content of the melted pyrometallurgical slag in step S1 is >30%, and the melting temperature of the pyrometallurgical slag is >1200°C.
[0008] Preferably, in step S1, when T>1600°C, the stirring rate is 5 r / min-10 r / min, and when 950°C<T≤1600°C, the stirring rate is 15 r / min-20 r / min.
[0009] Preferably, in step S1, the volume ratio of carbon dioxide in the carbon dioxide gas is greater than 70%, and the gas temperature is ≤200°C.
[0010] Preferably, in step S1, when T>1600°C, the cooling rate of the molten smelting slag is 0.5°C / min to 0.8°C / min, and when 950°C<T≤1600°C, the cooling rate of the molten smelting slag is 1°C / min to 1.5°C / min.
[0011] Preferably, during the cooling process of step S2, the surface temperature of the smelting slag reaches 900°C~950°C, which is regarded as reaching the end point of slow cooling, and carbonized smelting slag is obtained. Thereafter, the carbonized smelting slag is placed in a stockpile through 15 m³~20 m³ slag packaging bags, and mobile water mist cooling is used to continue cooling the carbonized smelting slag to room temperature.
[0012] Beneficial effects of the present invention: 1. The present invention uses carbon dioxide gas to purge and slowly cool the molten pyrometallurgical slag. The slow cooling process converts silicate minerals into carbonate minerals and generates silicon dioxide, thereby reducing the viscosity and fluidity of the molten smelting slag and promoting the growth of crystals such as iron and copper. The present invention strengthens the carbon fixation effect of the alkaline pyrometallurgical slag, with a carbon dioxide fixation rate of >85%, achieving phase reconstruction and carbon fixation, and facilitating the improvement of subsequent separation rate and recovery rate of copper and iron metals. The method of the present invention has high economic benefits and can be put into practical industrial applications. 2. The present invention not only solves the technical problems of high energy consumption, large water consumption, long slow cooling time, etc. existing in the current air slow cooling and water quenching slow cooling processes, but also can realize carbon capture and carbon emission reduction in the pyrometallurgical process, promote the aggregation and crystallization of various metal crystals, and truly realize the reduction, resource utilization and harmlessness of pyrometallurgical slag. DETAILED DESCRIPTION
[0013] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0014] Example 1 The method for slowly cooling and carbonizing slag from pyrometallurgical process in this embodiment comprises the following steps: S1. Purge and slow cool the molten pyrometallurgical slag: introduce carbon dioxide gas into a high-temperature stirring tank to purge and slowly cool the molten pyrometallurgical slag to obtain carbonized smelting slag; the silicate content of the molten copper smelting slag is 53%, the melting temperature is 1350°C, the volume ratio of carbon dioxide gas is 75%, the gas temperature is 200°C, and the stirring speed is 15r / min; S2. Water quenching of carbonized smelting slag: Cool the carbonized smelting slag to room temperature by water cooling; wherein, the slow cooling rate of the smelting slag is 1.2℃ / min, and the carbonized smelting slag is slowly cooled to 930℃ to obtain the carbonized smelting slag. After the carbonized smelting slag is loaded into a 20m³ slag bag, it is placed in the yard and the mobile water mist cooling is used to continue to cool the carbonized smelting slag to 30℃; The carbon dioxide concentration in the inlet and outlet gases was continuously detected online and the carbon dioxide fixation rate was calculated. In this embodiment, the carbon dioxide fixation rate was 87%. The obtained copper smelting slag was electronically scanned, and the particle size distribution range of metallic copper was 0.25 mm ~ 0.3 mm, which was about 63% higher than that of water quenching and slow cooling, and about 30% higher than that of air slow cooling. The particle size distribution range of metallic iron was 0.15 mm ~ 0.17 mm, which was about 57% higher than that of water quenching and slow cooling, and about 38% higher than that of air slow cooling.
[0015] Example 2 The method for slowly cooling and carbonizing slag from pyrometallurgical process in this embodiment comprises the following steps: S1. Purge and slow cool the molten pyrometallurgical slag: introduce carbon dioxide gas into a high-temperature stirring tank to purge and slowly cool the molten pyrometallurgical slag to obtain carbonized smelting slag; the silicate content of the molten copper smelting slag is 53%, the melting temperature is 1350°C, the volume ratio of carbon dioxide gas is 79%, the gas temperature is 200°C, and the stirring speed is 17r / min; S2. Water quenching of carbonized smelting slag: Cool the carbonized smelting slag to room temperature by water cooling; wherein, the slow cooling rate of the smelting slag is 1.2℃ / min, and the carbonized smelting slag is slowly cooled to 900℃ to obtain the carbonized smelting slag. After the carbonized smelting slag is loaded into a 20m³ slag bag, it is placed in the stockpile and the mobile water mist cooling is used to continue to cool the carbonized smelting slag to 25℃; The carbon dioxide concentration in the inlet and outlet gases was continuously detected online and the carbon dioxide fixation rate was calculated. In this embodiment, the carbon dioxide fixation rate was 92%. The obtained copper smelting slag was electronically scanned, and the particle size distribution range of metallic copper was 0.27 mm ~ 0.28 mm, which was about 80% higher than that of water quenching and slow cooling, and about 42% higher than that of air slow cooling. The particle size distribution range of metallic iron was 0.17 mm ~ 0.18 mm, which was about 88% higher than that of water quenching and slow cooling, and about 54% higher than that of air slow cooling.
[0016] Example 3 The method for slowly cooling and carbonizing slag from pyrometallurgical process in this embodiment comprises the following steps: S1. Purge and slow cooling of molten pyrometallurgical slag: introduce carbon dioxide gas into a high-temperature stirring tank, purge and slow cool the molten pyrometallurgical slag to obtain carbonized smelting slag; the silicate content of the molten copper smelting slag is 62%, the melting temperature is 1732°C, the volume ratio of carbon dioxide gas is 82%, and the gas temperature is 200°C; when the temperature of the molten steel slag is >1600°C, the stirring speed of the stirring tank is 7r / min, and the slow cooling speed is 0.5°C / min; when the smelting slag temperature is ≤1600°C, the stirring speed of the stirring tank is 17r / min, and the slow cooling speed is 1.5°C / min; S2. Water quenching of carbonized smelting slag: slowly cooling to 900°C to obtain carbonized smelting slag, loading the carbonized smelting slag into a 20m³ slag bag, placing it in a stockpile, and using mobile water mist cooling to continue cooling the carbonized smelting slag to 25°C; The carbon dioxide concentration in the inlet and outlet gases was continuously detected online and the carbon dioxide fixation rate was calculated. In this embodiment, the carbon dioxide fixation rate was 95%. The obtained copper smelting slag was electronically scanned, and the metal copper particle size distribution range was 0.37 mm ~ 0.41 mm, which was about 90% higher than that of water quenching and slow cooling, and about 56% higher than that of air slow cooling. The metal iron particle size distribution range was 0.24 mm ~ 0.27 mm, which was about 93% higher than that of water quenching and slow cooling, and about 62% higher than that of air slow cooling.
[0017] Example 4 The method for slowly cooling and carbonizing slag from pyrometallurgical process in this embodiment comprises the following steps: S1. Purge and slow cooling of molten pyrometallurgical slag: introduce carbon dioxide gas into a high-temperature stirring tank, purge and slow cool the molten pyrometallurgical slag to obtain carbonized smelting slag; the silicate content of the molten copper smelting slag is 62%, the melting temperature is 1732°C, the volume ratio of carbon dioxide gas is 73%, and the gas temperature is 180°C; when the temperature of the molten steel slag is >1600°C, the stirring speed of the stirring tank is 5r / min, and the slow cooling speed is 0.7°C / min; when the smelting slag temperature is ≤1600°C, the stirring speed of the stirring tank is 20r / min, and the slow cooling speed is 1.7°C / min; S2. Water quenching of carbonized smelting slag: slowly cooling to 900°C to obtain carbonized smelting slag, loading the carbonized smelting slag into a 20m³ slag bag, placing it in a stockpile, and using mobile water mist cooling to continue cooling the carbonized smelting slag to 30°C; The carbon dioxide concentration in the inlet and outlet gases was continuously detected online and the carbon dioxide fixation rate was calculated. In this embodiment, the carbon dioxide fixation rate was 90%. The obtained copper smelting slag was electronically scanned, and the particle size distribution range of metallic copper was 0.34 mm ~ 0.36 mm, which was about 78% higher than that of water quenching and slow cooling, and about 36% higher than that of air slow cooling. The particle size distribution range of metallic iron was 0.22 mm ~ 0.24 mm, which was about 83% higher than that of water quenching and slow cooling, and about 57% higher than that of air slow cooling.
[0018] Through analysis of the embodiments, the method of the present invention can simultaneously realize carbon fixation and crystal growth of iron, copper, etc., under the preferred reaction conditions, the carbon dioxide fixation rate is above 85%, and the particle size of iron and copper is significantly increased compared with slow cooling by air and slow cooling by water quenching. It can be put into actual industrial application to realize the reduction, resource utilization and harmlessness of pyrometallurgical slag.
[0019] Example 5 This embodiment is based on Example 1, and the differences from Example 1 are: the volume ratio of carbon dioxide gas is 70.1%, the gas temperature is 180°C, and the stirring speed is 15r / min; the smelting slag slow cooling rate is 1°C / min, and it is slowly cooled to 900°C to obtain carbonized smelting slag.
[0020] Example 6 This embodiment is based on Example 1, and the differences from Example 1 are: the volume ratio of carbon dioxide gas is 75%, the gas temperature is 200°C, and the stirring speed is 20r / min; the smelting slag slow cooling rate is 1.5°C / min, and it is slowly cooled to 950°C to obtain carbonized smelting slag.
[0021] Example 7 This embodiment is based on Example 1, and the differences from Example 1 are: the volume ratio of carbon dioxide gas is 73%, the gas temperature is 190°C, and the stirring speed is 17.5r / min; the smelting slag slow cooling rate is 1.25°C / min, and it is slowly cooled to 925°C to obtain carbonized smelting slag.
[0022] Example 8 This embodiment is based on Example 3, and the difference from Example 3 is that when the temperature of molten steel slag is greater than 1600°C, the stirring speed of the stirring tank is 5 r / min, and the slow cooling speed is 0.5°C / min; when the temperature of smelting slag is less than 1600°C, the stirring speed of the stirring tank is 15 r / min, and the slow cooling speed is 1°C / min.
[0023] Example 9 This embodiment is based on Example 3, and the difference from Example 3 is that when the temperature of molten steel slag is greater than 1600°C, the stirring speed of the stirring tank is 10 r / min, and the slow cooling speed is 0.8°C / min; when the temperature of smelting slag is less than 1600°C, the stirring speed of the stirring tank is 20 r / min, and the slow cooling speed is 1.5°C / min.
[0024] Example 10 This embodiment is based on Example 3, and the difference from Example 3 is that when the temperature of molten steel slag is greater than 1600°C, the stirring speed of the stirring tank is 7.5 r / min, and the slow cooling speed is 0.65°C / min; when the temperature of smelting slag is less than 1600°C, the stirring speed of the stirring tank is 17.5 r / min, and the slow cooling speed is 1.25°C / min.
Claims
1. A method for slowly cooling and carbonizing slag from pyrometallurgical process, Features The following steps are involved: S1. Purging and slow cooling of molten pyrometallurgical slag: introducing carbon dioxide gas into a high-temperature stirring tank to purge and slowly cool the molten pyrometallurgical slag to obtain carbonized smelting slag; S2. Water quenching of carbonized smelting slag: cool the carbonized smelting slag to room temperature by water cooling.
2. The method for slowly cooling and carbonizing slag from pyrometallurgical process according to claim 1, Features The silicate mineral content of the melted pyrometallurgical slag in step S1 is >30%, and the melting temperature of the pyrometallurgical slag is >1200°C.
3. The method for slowly cooling and carbonizing slag from pyrometallurgical process according to claim 1, Features In step S1, when T>1600℃, the stirring rate is 5 r / min ~10 r / min, and when 950℃<T≤1600℃, the stirring rate is 15 r / min ~20 r / min.
4. The method for slowly cooling and carbonizing slag from pyrometallurgical process according to claim 1, Features In step S1, the volume ratio of carbon dioxide in the carbon dioxide gas is greater than 70%, and the gas temperature is less than or equal to 200°C.
5. The method for slowly cooling and carbonizing slag from pyrometallurgical process according to claim 1, Features In step S1, when T>1600°C, the cooling rate of the molten smelting slag is 0.5°C / min to 0.8°C / min, and when 950°C<T≤1600°C, the cooling rate of the molten smelting slag is 1°C / min to 1.5°C / min.
6. The method for slowly cooling and fixing carbon in pyrometallurgical slag according to claim 1, Features During the cooling process of step S2, when the surface temperature of the smelting slag reaches 900℃~950℃, it is considered to reach the end point of slow cooling, and carbonized smelting slag is obtained. After that, the carbonized smelting slag is placed in the yard through 15 m³~20 m³ slag packaging bags, and mobile water mist cooling is used to continue to cool the carbonized smelting slag to room temperature.