Treatment process of high-palladium anode slime
By adding extraction steps and gradual heating and calcining to the high-palladium anode mud treatment process, combined with the use of acid solution and catalyst, the problem of copper anode mud treatment with excessive palladium element content is solved, and the recovery rate of palladium element and the purity of precious metals are improved. , achieving a safe and efficient separation effect.
Patent Information
- Application Number
- CN202411023888.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing gold chloride separation method is difficult to treat copper anode mud with excessive palladium content, resulting in excessive palladium residue and low direct yield.
The extraction step is added to the treatment process, the precipitate is put into triisobutylphosphine sulfide, dissolves the palladium element, and isolates precious metals such as palladium, gold, platinum, and silver by gradually heating and calcining, using acid solution and catalyst, and improves the Recovery and purity.
The recovery rate of palladium and the purity of precious metals are significantly improved, ensuring the reduction of palladium content, making the separation in subsequent steps more efficient, and avoiding equipment damage and operation risks.
Smart Images

Figure BDA0004968016010000061
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical technology, and in particular to a treatment process for high-palladium anode mud. Background Art
[0002] Palladium is a silvery white precious metal with good physical and chemical properties. It is widely used in industrial production and high-tech fields. Its main uses are as follows: 1. Automobile industry: Palladium is one of the important components of the three-way catalytic converter, which can convert harmful substances in automobile exhaust into harmless substances and purify the environment.
[0003] 2. Electronics industry: Palladium is an important raw material for capacitors, resistors, sockets, connectors and other components. Mixed palladium-silver alloy and palladium-iridium alloy can be used to manufacture high-speed read-write heads.
[0004] 3. Chemical industry: Palladium is an important catalyst for the production of ethylene, LCD TVs, artificial gemstones, etc. It can also be used to manufacture inkjet printer inks, etc.
[0005] Copper anode mud contains a lot of palladium. How to efficiently recover the palladium in copper anode mud has attracted widespread attention. The existing technical treatment methods are: 1. Sulfate the anode mud in a certain proportion and add it into the muffle furnace for roasting at different stage temperatures.
[0006] 2. Copper separation: After roasting, the slag is ball-milled and slurried, then placed in a reactor for water leaching to separate copper and acid leaching to separate tellurium.
[0007] 3. Gold separation: Under acidic conditions, sodium chlorate is added to chlorinate the gold. After the gold separation process, it is reduced with sodium sulfite to obtain gold, platinum and palladium crude powder, which is then purified and refined.
[0008] 4. Silver separation: After gold separation, the solid residue is treated with sodium carbonate to remove lead, and ammonia to separate the silver.
[0009] However, the existing chlorination gold separation method is difficult to treat copper anode mud with too high palladium content. Using the existing method to treat copper anode mud with too high palladium content will cause excessive palladium residue in the solid slag, resulting in a low direct recovery rate. Therefore, it is necessary to develop a treatment process that can cope with copper anode mud with too high palladium content. Summary of the invention
[0010] In order to improve the recovery rate of palladium element and the yield and purity of precious metals when treating copper anode mud with a high palladium content, the present application provides a treatment process for high-palladium anode mud.
[0011] The present application provides a high-palladium anode mud treatment process, comprising the following steps: S1. Anode mud roasting: After anode mud and sulfuric acid are mixed in a certain proportion, the mixture is stirred and reacted at a speed of 60r / min for 2-3 hours. After the reaction is complete, the slurry is transported to a muffle furnace for roasting to obtain slag; S2, separation of copper: placing the slag obtained in step S1 in deionized water, stirring and reacting for 0.5-1 hour at a speed of 60 r / min, standing after the stirring to obtain a supernatant and a precipitate, washing the precipitate with deionized water for multiple times, mixing the washing liquid and the supernatant and vacuum drying to obtain copper sulfate; S3, tellurium separation: the precipitate obtained in step S2 is put into an acid solution, a catalyst is added, and the reaction is continuously stirred at a speed of 60 r / min for 0.5-1 hour. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate. The precipitate is rinsed with an acid solution for multiple times, and the rinse liquid and the supernatant are mixed and then vacuum dried to obtain tellurium oxide.
[0012] S4, extraction: putting the precipitate obtained in step S3 into an acid solution of triisobutylphosphine sulfide, stirring and reacting for 0.5-1 hour at a speed of 60 r / min, standing after the stirring to obtain a supernatant and a precipitate, washing the precipitate with an acid solution for multiple times, mixing the washing liquid and the supernatant and vacuum drying to obtain a palladium salt; S5, separation of gold: putting the precipitate obtained in step S4 into an acid solution, adding an oxidant, stirring and reacting at a speed of 60 r / min for 1-2 hours, standing after the stirring is completed to obtain a supernatant and a precipitate, washing the precipitate with an acid solution for multiple times, mixing the washing liquid and the supernatant, adding a reducing agent, stirring and reacting at a speed of 60 r / min for 1-2 hours, filtering and drying after the reaction is completed to obtain gold powder and platinum powder; S6, separation of silver: putting the precipitate obtained in step S5 into a sodium carbonate solution, stirring and reacting at a speed of 60 r / min for 1-2 hours, standing after stirring to obtain a supernatant and a precipitate, putting the precipitate into a hydrochloric acid solution, stirring and reacting at a speed of 60 r / min for 0.5-1 hour, filtering after the reaction is complete, putting the precipitate into ammonia water, stirring and reacting at a speed of 60 r / min for 1-2 hours, filtering after the reaction is complete, and obtaining silver powder.
[0013] By adopting the above technical scheme, the biggest difference between the present application and the traditional treatment process when treating anode mud is that an extraction process is added before the gold separation step. By placing the precipitate in triisobutylphosphine sulfide, the triisobutylphosphine sulfide plays a role in dissolving the palladium element, and more palladium elements in the mixture are dissolved in the solvent, so that the palladium content in the precipitate is greatly reduced, so that the precipitate meets the requirements of the traditional treatment process, and thus the traditional process is continued for treatment, which not only greatly improves the recovery rate of the palladium element, but also improves the purity and yield of the precious metals recovered in the subsequent steps.
[0014] In the present application, the organic matter in the copper anode mud is removed by mixing the copper anode mud with sulfuric acid and then roasting it, and the metal elements are converted into the form of sulfates. Therefore, in the subsequent copper separation process, deionized water can be simply used to dissolve copper sulfate, thereby conveniently removing the copper element with a high content and facilitating the subsequent separation of other elements.
[0015] In the present application, under the action of an acid solution and a catalyst, the tellurium element in the precipitate is converted into tellurate ions and dissolved in the solution, thereby separating the tellurium element from the precipitate. Subsequently, the tellurium element is evaporated from the solvent by vacuum drying to form tellurium oxide solid. This separation method is not only simple to operate, but also has a high degree of separation.
[0016] Gold and platinum are difficult to leach using ordinary solutions due to their weak activity. In this application, a variety of elements such as gold, platinum, and silver are first dissolved in a solution using a strong oxidant in an acidic environment. After dissolution, the metal ions are reduced by a reducing agent. Due to the weak activity of gold and platinum, they will be preferentially reduced to a metallic solid state, thereby achieving the separation of precious metals. This separation method has a high degree of separation.
[0017] Lead and silver are difficult to separate by general methods due to their similar reactivity. In the present application, lead sulfate in the precipitate is converted into lead carbonate by leaching with sodium carbonate solution, while silver sulfate is difficult to be converted due to its low solubility and remains in the state of silver sulfate. Lead carbonate reacts with hydrochloric acid, so that the lead element is dissolved in the solution, while the silver element remains in a solid state. Finally, ammonia water is used to obtain silver powder. This separation method has a high separation degree.
[0018] In the present invention, the mass ratio of anode mud to sulfuric acid in step S1 is 1:(0.5-1).
[0019] By adopting the above technical solution, in this application, through multiple experiments by operators, it is found that the mass ratio of anode mud to sulfuric acid is 1: (0.5-1) which is more suitable. When the amount of sulfuric acid is too little, it is difficult to convert most of the metal elements into sulfates, resulting in a significant decrease in the yield. When the amount of sulfuric acid is too much, the solution forms a suspension instead of mud, and the dilute liquid is prone to danger when roasting in a muffle furnace. .
[0020] In the present invention, the calcination method in step S1 is first calcining at 350-400°C for 1 hour, then calcining at 500-550°C for 1 hour, and finally calcining at 600-650°C for 1 hour.
[0021] By adopting the above technical solution, the copper anode mud contains more organic matter, and when roasted at high temperature, it is easy to produce a large amount of gas in a short time, which can easily cause equipment damage and injury to operators. In this application, the gas generation speed is slower and safer by gradually increasing the temperature during roasting.
[0022] In the present invention, the acid solution in step S3 is one or a combination of hydrochloric acid and sulfuric acid, and the catalyst in step S3 is one or a combination of sodium chloride, potassium chloride and sodium hypochlorite.
[0023] By adopting the above technical solution, in the present application, the chloride ions mainly play a catalytic effect in step S3. In order for the chloride ions to have a better catalytic effect, they need to be catalyzed in an acidic environment. Therefore, the present application screened acid solutions and chlorides. Sodium hypochlorite can not only provide chloride ions after hydrolysis, but also provide a certain oxidizing property. The catalytic effect in the present application is relatively excellent.
[0024] In the present invention, the acid solution in step S4 is one or a combination of hydrochloric acid, sulfuric acid and nitric acid.
[0025] By adopting the above technical solution, in the present application, the reaction in step S4 needs to be carried out in an acidic environment. Sulfuric acid and hydrochloric acid can increase the acidity, while nitric acid can not only provide acidity but also has strong oxidizing properties, and performs better in the present application.
[0026] In the present invention, the acid solution in step S5 is one or a combination of hydrochloric acid and sulfuric acid, the oxidant in step S5 is one or a combination of hydrogen peroxide, sodium hypochlorite, sodium chlorate and potassium permanganate, and the reducing agent in step S5 is sodium sulfite.
[0027] By adopting the above technical solution, the oxidant in this application needs to be in an acidic environment to exert a strong oxidizing effect. Therefore, the operator screened suitable acids and oxidants through multiple experiments. In the subsequent reduction process, if the reducing effect of the reducing agent is strong, it is easy to reduce metal elements such as gold and platinum to metal powder, which reduces the purity of the precious metals. Through multiple experiments by the operator, it was found that in this application, it is more appropriate to use sodium sulfite as the reducing agent.
[0028] In the present invention, the extractant triisobutylphosphine sulfide in step S4 is prepared by reacting triisobutylphosphine with elemental sulfur in a benzene solvent.
[0029] In the present invention, the molar ratio of triisobutylphosphine to elemental sulfur is 1:(1.05-1.2).
[0030] By adopting the above technical solution, the excessive addition of sulfur can ensure that triisobutylphosphine is completely reacted, thereby reducing the waste of raw materials.
[0031] In summary, the present application includes at least one of the following beneficial technical effects: 1. When treating anode mud, the biggest difference between the present application and the traditional treatment process is that an extraction process is added before the gold separation step. By placing the precipitate in triisobutylphosphine sulfide, triisobutylphosphine sulfide plays a role in dissolving palladium elements, and more palladium elements in the mixture are dissolved in the solvent, so that the palladium content in the precipitate is greatly reduced, so that the precipitate meets the requirements of the traditional treatment process, and thus the traditional process is continued for treatment, which not only greatly improves the recovery rate of palladium elements, but also improves the purity and yield of precious metals recovered in subsequent steps.
[0032] 2. Copper anode mud contains more organic matter. When roasted at high temperature, it is easy to produce a large amount of gas in a short time, which can easily cause equipment damage and harm to operators. In this application, the gas generation speed is slower and safer by gradually increasing the temperature during roasting.
[0033] 3. In the present application, the main catalytic effect in step S3 is chloride ion, and in order for chloride ion to have a better catalytic effect, it is necessary to catalyze in an acidic environment. Therefore, the present application screened acid solutions and chlorides, and sodium hypochlorite can not only provide chloride ions after hydrolysis, but also provide a certain oxidizing property, and the catalytic effect in the present application is relatively excellent. DETAILED DESCRIPTION
[0034] The present application is further described in detail below in conjunction with the specific contents. Example
[0035] Example 1 A process for treating high-palladium anode mud comprises the following steps: S1. Anode mud roasting: 100g of high palladium anode mud and 100g of sulfuric acid are mixed in a certain proportion, and the mixture is stirred and reacted for 2-3 hours at a speed of 60r / min. After the reaction is complete, the slurry is transported to a muffle furnace, and roasted at 350-400°C for 1 hour, then at 500-550°C for 1 hour, and finally at 600-650°C for 1 hour to obtain slag; S2, separation of copper: placing the slag obtained in step S1 in 500 ml of deionized water, stirring and reacting for 0.5-1 hour at a speed of 60 r / min, standing after the stirring to obtain a supernatant and a precipitate, washing the precipitate with deionized water for multiple times, mixing the washing liquid and the supernatant and vacuum drying to obtain copper sulfate; S3. Tellurium separation: the precipitate obtained in step S2 is put into 200 ml of 10% hydrochloric acid solution, 5 g of sodium chloride is added, and the reaction is continuously stirred at a speed of 60 r / min for 0.5-1 hour. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate. The precipitate is rinsed with an acid solution for multiple times, and the rinse liquid and the supernatant are mixed and then vacuum dried to obtain tellurium oxide.
[0036] S4, extraction: the precipitate obtained in step S3 is put into 100 ml of 10% nitric acid solution of triisobutylphosphine sulfide, and the mixture is stirred and reacted at a speed of 60 r / min for 0.5-1 hour. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate, and the precipitate is rinsed with an acid solution for multiple times. The rinse liquid and the supernatant are mixed and then vacuum dried to obtain a palladium salt; S5, separation of gold: the precipitate obtained in step S4 is put into 100 ml of 20% sulfuric acid solution, 20 g of sodium chlorate is added, and the mixture is stirred and reacted at a speed of 60 r / min for 1-2 hours. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate. The precipitate is rinsed with a 20% sulfuric acid solution for multiple times. After the rinse liquid and the supernatant are mixed, 20 g of sodium sulfite is added, and the mixture is stirred and reacted at a speed of 60 r / min for 1-2 hours. After the reaction is completed, the mixture is filtered and dried to obtain gold powder and platinum powder; S6, silver separation: the precipitate obtained in step S5 is put into 100 ml 10% sodium carbonate solution, and the mixture is stirred and reacted at a speed of 60 r / min for 1-2 hours. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate. The precipitate is put into an excess hydrochloric acid solution, and the mixture is stirred and reacted at a speed of 60 r / min for 0.5-1 hour. After the reaction is complete, the mixture is filtered. The precipitate is put into ammonia water, and the mixture is stirred and reacted at a speed of 60 r / min for 1-2 hours. After the reaction is complete, the mixture is filtered to obtain silver powder.
[0037] The difference between Comparative Example 1 and Example 1 is that there is no extraction process in step S4.
[0038] The difference between Examples 2 and 3 and Example 1 is that the acid used in step S4 is different, as shown in the following table: acid Example 1 Nitric acid Example 2 hydrochloric acid Example 3 sulfuric acid The difference between Examples 4, 5 and Comparative Example 2 and Example 1 is that the types of acid and catalyst used in step S3 are different, as shown in the following table: acid catalyst Example 1 hydrochloric acid Sodium chloride Example 4 sulfuric acid Sodium chloride Example 5 hydrochloric acid Sodium hypochlorite Comparative Example 2 Deionized water Sodium chloride Performance testing The purity and yield of the products obtained in each embodiment and comparative example were calculated as follows: Purity: The product of each example and comparative example was dissolved in a corresponding solvent and titrated to calculate the purity of the product.
[0039] Yield: Calculate the corresponding yield based on the purity of the product.
[0040] The test results are shown in the following table: Conclusion: It can be seen from the data of Example 1 and Comparative Example 1 in the above table that when the present application processes high-palladium anode mud, the purity of the recovered precious metals is greatly improved compared with the traditional process. This is because in the traditional recovery process, the palladium element in the anode mud will be separated together during the gold separation step, so that the metallic palladium is mixed in the precious metal powder, resulting in a decrease in the purity of the precious metal. In the present application, an extraction process is added before the gold separation process, and the palladium element in the anode mud is extracted by triisobutylphosphine sulfide, so that the palladium content in the anode mud is greatly reduced, so that when the subsequent gold separation process is carried out, the amount of palladium element taken out is greatly reduced, and the purity of the precious metal is significantly improved. Palladium element yield (%) Palladium purity (%) Example 1 98 99.5 Example 2 96 99.3 Example 3 94 99.3
[0041] Conclusion: It can be seen from the data of Examples 1, 2 and 3 in the above table that when the present application extracts the palladium element in step S4, the use of nitric acid as a solvent has a better recovery effect on the palladium element than hydrochloric acid and sulfuric acid. This is because nitric acid has a strong oxidizing property and can oxidize the solid palladium element in the anode mud into palladium ions, thereby significantly improving the yield of the palladium element. Purity of Selenium Tellurium Mixture (%) Selenium-tellurium mixture fine product yield (%) Example 1 99.5 95 Comparative Example 3 86.3 94
[0042] Conclusion: It can be seen from the data of Example 1 and Comparative Example 3 in the above table that the addition of sulfide salt in step S2 in the present application can greatly improve the purity of the product. This is because by adding sulfide salt to the solution, the metal ions in the solution react with the sulfide ions to form sulfide precipitates, thereby facilitating the removal of metal ions and thus improving the purity of the product. Tellurium element yield (%) Tellurium element purity (%) Example 1 96.2 99.7 Example 4 93.2 99.1 Example 5 97.5 99.6 Comparative Example 2 86.3 96.1
[0043] Conclusion: It can be seen from the data of Examples 1, 4, 5 and Comparative Example 2 in the above table that in the tellurium separation process in step S3 of the present application, when the acid solution is hydrochloric acid and the catalyst is sodium hypochlorite, the yield and purity of the tellurium element are relatively high. This is because in this process, chloride ions mainly play a catalytic effect, and in order for chloride ions to have an excellent catalytic effect, they need to be catalyzed in an acidic environment. In Comparative Example 2, deionized water is used instead of hydrochloric acid, and no acidic environment is provided, which greatly reduces the yield and purity of the tellurium element. In Example 5, sodium hypochlorite is used as a catalyst. Sodium hypochlorite itself has strong oxidizing properties and produces chloride ions after decomposition, which makes it have a relatively excellent catalytic effect in the present application.
[0044] The above-mentioned specific implementation examples are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. Therefore, all equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A process for treating high-palladium anode mud, characterized by: The steps include: S1. Anode mud roasting: After anode mud and sulfuric acid are mixed in a certain proportion, the mixture is stirred and reacted at a speed of 60r / min for 2-3 hours. After the reaction is complete, the slurry is transported to a muffle furnace for roasting to obtain slag; S2, separation of copper: placing the slag obtained in step S1 in deionized water, stirring and reacting for 0.5-1 hour at a speed of 60 r / min, standing after the stirring to obtain a supernatant and a precipitate, washing the precipitate with deionized water for multiple times, mixing the washing liquid and the supernatant and vacuum drying to obtain copper sulfate; S3, tellurium separation: the precipitate obtained in step S2 is put into an acid solution, a catalyst is added, and the mixture is stirred at a speed of 60 r / min for 0.5-1 hour. After the stirring is completed, the mixture is allowed to stand to obtain a supernatant and a precipitate. The precipitate is rinsed with an acid solution for multiple times, and the rinse liquid and the supernatant are mixed and then vacuum dried to obtain tellurium oxide; S4, extraction: putting the precipitate obtained in step S3 into an acid solution of triisobutylphosphine sulfide, stirring and reacting for 0.5-1 hour at a speed of 60 r / min, standing after the stirring to obtain a supernatant and a precipitate, washing the precipitate with an acid solution for multiple times, mixing the washing liquid and the supernatant and vacuum drying to obtain a palladium salt; S5, separation of gold: putting the precipitate obtained in step S4 into an acid solution, adding an oxidant, stirring and reacting at a speed of 60 r / min for 1-2 hours, standing after the stirring is completed to obtain a supernatant and a precipitate, washing the precipitate with an acid solution for multiple times, mixing the washing liquid and the supernatant, adding a reducing agent, stirring and reacting at a speed of 60 r / min for 1-2 hours, filtering and drying after the reaction is completed to obtain gold powder and platinum powder; S6, separation of silver: putting the precipitate obtained in step S5 into a sodium carbonate solution, stirring and reacting at a speed of 60 r / min for 1-2 hours, standing after stirring to obtain a supernatant and a precipitate, putting the precipitate into a hydrochloric acid solution, stirring and reacting at a speed of 60 r / min for 0.5-1 hour, filtering after the reaction is complete, putting the precipitate into ammonia water, stirring and reacting at a speed of 60 r / min for 1-2 hours, filtering after the reaction is complete, and obtaining silver powder.
2. A process for treating high-palladium anode mud according to claim 1, characterized in that: The mass ratio of anode mud to sulfuric acid in step S1 is 1:(0.5-1).
3. The process for treating high-palladium anode mud according to claim 1, characterized in that: The calcination method in step S1 is to firstly calcine at 350-400°C for 1 hour, then calcine at 500-550°C for 1 hour, and finally calcine at 600-650°C for 1 hour.
4. The process for treating high-palladium anode mud according to claim 1, characterized in that: The acid solution in step S3 is one or a combination of hydrochloric acid and sulfuric acid, and the catalyst in step S3 is one or a combination of sodium chloride, potassium chloride and sodium hypochlorite.
5. The process for treating high-palladium anode mud according to claim 1, characterized in that: The acid solution in step S4 is one or a combination of hydrochloric acid, sulfuric acid and nitric acid.
6. The process for treating high-palladium anode mud according to claim 1, characterized in that: The acid solution in step S5 is one or a combination of hydrochloric acid and sulfuric acid, the oxidant in step S5 is one or a combination of hydrogen peroxide, sodium hypochlorite, sodium chlorate and potassium permanganate, and the reducing agent in step S5 is sodium sulfite.
7. The process for treating high-palladium anode mud according to claim 1, characterized in that: The extractant triisobutylphosphine sulfide in step S4 is prepared by reacting triisobutylphosphine with elemental sulfur in a benzene solvent.
8. The process for treating high-palladium anode mud according to claim 1, characterized in that: The molar ratio of triisobutylphosphine to elemental sulfur is 1:(1.05-1.2).